Meaning
A coil is the wound strip that a mill rolls, tests and ships, and from which sheets are cut and dies are fed. Each coil comes from one production lot and carries its own certificate. Sheets cut from it share its thickness, strength and surface. Two coils of the same grade are therefore close, but never identical.Size and Mass
ArcelorMittal’s tables show how a coil is described. A coil of 25 tonnes (27.6 short tons) at 1,250 mm (49 in) wide has an inside diameter of 762 mm (30 in). Its outside diameter then comes to 1,960 mm (77 in). The tables also state coil mass per meter of width, here 20 t/m. A progressive die for a small bracket is fed from a narrower strip slit from such a coil.Read More
Mill Testing
Coating and tolerance tests belong to the coil, not to each part cut from it. For galvanized sheet, the triple spot test is taken edge, center and edge across the full-width coil. GalvInfo notes that a narrow sheet cut from it carries only the single spot guarantee. The certificate therefore reports the coil’s test, not each blank. A coil can pass on the triple spot average and still fail one edge reading.Coil to Coil
A repeat order may come from a different heat and a different mill. Measured thickness on the first sheet shows where one coil sits inside its EN 10131 band. The band shows how far the next coil may move. Two coils of the same grade also differ in yield strength. A part bent from the second coil can open half a degree from the first.Effect on Bending
The coil change reaches the bend angle before anything else. A batch cut in two sittings from two coils can differ in springback by a fraction of a degree. The first piece of the second coil is therefore checked as the first piece of the first. On a running die, a new coil lot is one of three events that call for a re-check. The other two are die sharpening and a press or feed change.Finish Match
Coils also differ in appearance. Euro Inox advises using coils from one production batch where large areas of sheeting share one elevation. Color consistency can vary from batch to batch. A cut and bent enclosure with several panels faces the same problem on a small scale. Panels cut from two coils can read as two finishes side by side.Flatness and Waves
The EN 10131 flatness tables apply to sheet, not to coil. Edge waves along the strip are limited separately, as a share of their length. The standard does not say how wide the wavy edge strip is. That width is found by a trial on the actual coil. A nest that keeps parts out of the outer strip avoids the worst of the wave.Record Keeping
A coil’s identity matters only if it travels with the parts. The job record of a batch therefore names the material lot with the nest and the first-piece measurement. A remnant without its certificate cannot be used for traced parts. A repeat batch is then cut from the record, so its first piece can be compared with the old part.