DrawingThin SheetWeld

ISO 5817 Weld Quality Levels B, C and D for Sheet Metal Parts

Name a quality level per joint, cite the current edition, and agree how thin-sheet welds are inspected and finished.

Three welded stainless steel sheet T-joints with weld beads of different quality, one smooth and even, one uneven and ropey, one with spatter beside it.

On a 2 mm sheet, ISO 5817 lets two plates sit out of line by 0.4 mm in a level B weld, 0.5 mm in level C and 0.7 mm in level D. The whole spread between the best and the loosest level is 0.3 mm, and the same sheet gets no allowance at all for an undercut at level B while level D accepts one up to 0.4 mm deep. Those few tenths of a millimeter are what a quality level buys on thin material, and a drawing that names no level leaves all of them open.

The standard reads like a long table, and for sheet metal only part of it bites.

What Quality Levels B, C and D Mean for a Sheet Metal Weld

ISO 5817 specifies quality levels for imperfections in fusion-welded joints in steel, nickel, titanium and their alloys. It applies to material 0.5 mm thick and above and covers fully penetrated butt welds and all fillet welds. Three levels are given, named D, C and B, and B is the highest requirement on the finished weld.

Each level is a list of limits for named imperfections: cracks, pores, undercut, misalignment, excess weld metal and so on. The levels are cumulative in effect. Anything permitted at B is permitted at C and D, and the limits tighten from D through C to B. The standard describes its levels as referring to production and good workmanship, and it says they are not tied to any particular application.

For a part under 3 mm, the standard gives separate limits, written as fractions of the sheet thickness t. That is the reason the numbers on thin sheet are so small: the allowed depth of an undercut at level C is one tenth of t, so a 1.5 mm sheet allows 0.15 mm.

ISO 5817 sorts weld imperfections into three levels, D, C and B, with B the strictest. On sheet under 3 mm the limits are fractions of the thickness, so each level is measured in tenths of a millimeter.

What ISO 5817 Covers and What It Leaves Open

The standard applies to manual, mechanized and automatic welding in all positions, and to butt welds, fillet welds and branch connections. Its listed processes, named by their ISO 4063 numbers, are metal arc welding without gas protection (11), submerged arc (12), gas-shielded metal arc (13), tungsten inert gas (14), plasma arc (15) and oxyfuel gas welding for steel only (31). Beam welding is excluded, and the standard sends laser and electron beam welds to ISO 13919-1.

That exclusion matters for sheet shops, because laser welding of thin sheet is common. A part welded by laser takes its levels from the beam welding standard, and a drawing that cites ISO 5817 for a laser seam has cited the wrong document.

The standard is also candid about what it does not do.

  • Metallurgical aspects, such as grain size and hardness, are not covered.
  • Which level a product needs is not stated. That choice goes to the application standard or to the designer working with the manufacturer and user.
  • How to detect imperfections is not described, and ISO 17635 is named as the document that correlates levels with acceptance levels for the different non-destructive methods.
  • The unit is the joint type in fabrication and not the whole product, so one part can carry different levels on different joints.
  • Fitness for purpose is outside the main part, and an annex gives extra criteria for fatigue.

The limits sit in one long table of four groups: surface imperfections, internal imperfections, imperfections in joint geometry and multiple imperfections. Internal gas porosity shows the pattern in miniature. For uniformly distributed porosity in a single layer, the projected area limit is 2.5 % at level D, 1.5 % at C and 1 % at B, and for multiple layers 5 %, 3 % and 2 %.

Thickness splits most rows at 3 mm, and the sheet metal reader lives in the rows for 0.5 to 3 mm. Below 0.5 mm the standard offers nothing, so a foil-thin part agrees its acceptance directly with the fabricator. Above 3 mm the formulas gain ceilings in millimeters, such as 0.5 mm of undercut depth at level C, and a 4 mm sheet is judged by a different row than a 3 mm one.

Aluminum is outside the scope as written. The standard names steel, nickel, titanium and their alloys, and a welded aluminum part needs a quality level from a different document.

Limits That Decide a Thin Sheet Weld

For thicknesses from 0.5 to 3 mm, the limits that most often decide a part are the ones in Table 1. They are written in ISO 5817 as formulas of the nominal thickness t, the nominal butt weld thickness s or the throat thickness a, and the table also gives the worked value on a 2 mm sheet with a fillet throat a of 2 mm.

Table 1. ISO 5817:2023 limits for thin material (0.5 to 3 mm) by quality level, with the worked value for t = 2 mm; “none” means not permitted
Imperfection Level D Level C Level B Worked value at t = 2 mm (D, C, B)
Surface pore, single, butt weld d ≤ 0.3 s none none 0.6 mm at D with s = 2 mm; none at C or B
Continuous or intermittent undercut, short h ≤ 0.2 t h ≤ 0.1 t none 0.4 mm, 0.2 mm, none
Shrinkage groove, short h ≤ 0.1 t + 0.2 mm h ≤ 0.1 t none 0.4 mm, 0.2 mm, none
Root concavity h ≤ 0.1 t + 0.2 mm h ≤ 0.1 t, short none 0.4 mm, 0.2 mm, none
Sagging, short h ≤ 0.25 t h ≤ 0.1 t none 0.5 mm, 0.2 mm, none
Linear misalignment between plates h ≤ 0.25 t + 0.2 mm h ≤ 0.15 t + 0.2 mm h ≤ 0.1 t + 0.2 mm 0.7 mm, 0.5 mm, 0.4 mm
Insufficient throat thickness, short h ≤ 0.1 a + 0.2 mm h ≤ 0.2 mm none 0.4 mm, 0.2 mm, none with a = 2 mm
Root gap, fillet weld h ≤ 0.1 aA + 0.5 mm h ≤ 0.1 aA + 0.3 mm h ≤ 0.1 aA + 0.2 mm 0.7 mm, 0.5 mm, 0.4 mm with aA = 2 mm

Two patterns stand out. The misalignment limit keeps a value at level B, because plates cannot be held in perfect register, and its fixed 0.2 mm term makes the thinner plate the one that suffers: at 0.8 mm, level B allows 0.28 mm, about a third of the sheet thickness. Short imperfection limits, on the other hand, disappear at B for undercut, shrinkage grooves, concavity and sagging. A level B weld on thin sheet is a weld with none of these defects.

The standard defines “short” in a specific way. For a weld 100 mm long or longer, a short imperfection is one whose total length is no more than 25 mm in the 100 mm of weld holding the most imperfections. Under 100 mm of weld length, it is no more than 25 % of the weld length. Two imperfections that sit closer than the major dimension of the smaller one count as one.

Imperfections With No Allowance at Levels C and B

Some imperfections get no allowance at any level, and others lose theirs at C or B. A drawing that names a level silently names every item on this list as a rejection.

  • Cracks, crater cracks, surface lack of fusion and burn through are not permitted at D, C or B, in material 0.5 mm and thicker.
  • Surface pores, end crater pipes, overlap, poor restarts, root porosity and stray arcs have an allowance at D only, and none at C or B in thin material.
  • A visible oxide film (temper colors) and spatter have no fixed limit at any level, only a note that acceptance depends on the application, for instance the material and its corrosion protection.
  • Several imperfections in one cross-section are not permitted at any level for thickness 0.5 to 3 mm, according to the 2023 edition’s revised row on multiple imperfections.

A level is a promise about imperfections, not about appearance. Spatter and heat tint have no limit at any level, so the drawing has to carry them.

The last item changed in the fourth edition. Its foreword lists an exclusion of several imperfections and a change of acceptance criteria in that row, so a drawing that cites an older edition and one that cites ISO 5817:2023 may not describe the same inspection.

Internal imperfections have their own rows, and they matter when a seam is radiographed or sectioned. A single gas pore in a butt weld may be up to 0.4 s at level D, 0.3 s at C and 0.2 s at B, with ceilings of 5 mm, 4 mm and 3 mm. Clustered porosity is limited by the diameter of the circle that encloses the pores: 25 mm at D, 20 mm at C and 15 mm at B, or the weld width in the first two cases and half the weld width at B.

Linear porosity and elongated cavities in a butt weld are held to 0.4 s, 0.3 s and 0.2 s in height. Whether they are checked at all depends on the extent of testing the contract sets.

Weld Shape Limits for Reinforcement, Convexity and Penetration

The other group of limits concerns the shape of the finished seam, and these limits grow with the weld width b. Table 2 gives the formulas for the three, with the ceiling the standard sets.

Table 2. ISO 5817:2023 shape limits that apply from 0.5 mm thickness, by quality level (b is the width of the weld reinforcement or cap)
Feature Level D Level C Level B
Excess weld metal, butt weld h ≤ 0.25 b + 1 mm, max 10 mm h ≤ 0.15 b + 1 mm, max 7 mm h ≤ 0.1 b + 1 mm, max 5 mm
Excessive convexity, fillet weld h ≤ 0.25 b + 1 mm, max 5 mm h ≤ 0.15 b + 1 mm, max 4 mm h ≤ 0.1 b + 1 mm, max 3 mm
Excessive penetration, 0.5 to 3 mm h ≤ 0.6 b + 1 mm h ≤ 0.3 b + 1 mm h ≤ 0.1 b + 1 mm
Weld toe angle, butt weld α ≥ 90° α ≥ 110° α ≥ 150°
Weld toe angle, fillet weld α ≥ 90° α ≥ 100° α ≥ 110°

For a butt weld cap 6 mm wide, the table allows 2.5 mm of excess metal at D, 1.9 mm at C and 1.6 mm at B. The toe angle limit is the more telling one for appearance and fatigue: a butt weld at level B has to blend into the plate at 150° or flatter, which in practice means dressing or a smooth TIG pass. Its introduction makes the same point, noting that level B values may need extra work such as grinding or TIG dressing.

Penetration on the root side follows the same logic. On thin sheet, penetration beyond the plate on the back is limited to 0.1 b + 1 mm at level B, and a seam on a visible face therefore reads as a deliberate cosmetic requirement, not an accident.

Choosing a Level and Writing It on the Drawing

The standard asks that the level be prescribed before production starts, preferably at enquiry or order. Its introduction lists what to weigh in the choice: design considerations, subsequent processing such as surfacing, the mode of stressing (static or dynamic), service conditions such as temperature and environment, and the consequences of failure. It adds that economic factors count, and that they include the work of inspection, testing and repair as well as welding.

In practice, a drawing carries one level for the whole part and a different one for the joints that need it. An enclosure seam that is ground flush and painted may take level C, and a pressure-bearing or fatigue-loaded joint may call for level B, with the rest at D. The standard allows this, since levels apply to individual joints.

Annex B covers welds in steel under fatigue loading, and it extends the designation with the letters FAT. Table 3 lists the three fatigue-extended levels.

Table 3. Fatigue-extended quality level designations in ISO 5817:2023 Annex B
Designation Fatigue class Added to Remark
ISO 5817-C63 FAT 63 level C limits adjusted to FAT 63
ISO 5817-B90 FAT 90 level B limits adjusted to FAT 90
ISO 5817-B125 FAT 125 level B generally not achieved as welded; fillet welds excluded

Annex B does not apply to level D. A footnote also says the values were proved by the International Institute of Welding for a material thickness of 10 mm and above, and that lower thicknesses may be applicable. For sheet parts below 3 mm, the fatigue designations are therefore a starting point to agree with the fabricator, not a verified rating.

How a Weld Is Checked Against a Level

ISO 5817 is written to apply directly to visual testing. When macro-examination is used, only imperfections detectable with a tenfold magnification at most are considered, with micro lack of fusion and microcracks excluded from that rule. Micro lack of fusion is defined as detectable only at 50 times magnification or more and is permitted at D and C and not at B.

Several rules guide how an inspector reads a joint. A joint is assessed separately for each type of imperfection, and the combined limit for multiple imperfections applies only if each single limit is met. Systematic imperfections, which repeat along the weld length even though each one is within limits, are allowed only at level D. The standard also notes the difficulty of reading its limits through non-destructive methods such as ultrasonic, radiographic, eddy current, penetrant and magnetic particle testing, and says those will probably need supplementary requirements.

Cite the edition, give a level for each joint and name the inspection method. The standard supplies limits for imperfections, and the contract supplies everything else.

So a drawing that says level B and nothing more leaves a gap between the limits and the inspection method. The extent of testing, the method and the sampling belong in the contract, along with the quality level, and the standard says so itself.

A buyer ordering welded sheet parts should therefore state the level per joint, the edition of the standard, the method of inspection and the finishing that follows the weld. That is how a first run at low-volume sheet metal reaches the same weld quality that a later bridge production batch has to repeat.

Sources and Further Reading

Request a Sheet Metal Quote

Send the 2D drawing and the 3D file, with the quantity and the stage of the project. An engineer replies within 1 working day.

The quote form, the mutual NDA and the private folder for your files are on Protolis Atelier, with Sheet Metal chosen.

Request a Quote