A cold rolled sheet 1.5 mm thick and 1,250 mm wide, in a soft grade, can lie 8 mm (0.315 in) off flat on a table and still be a conforming delivery under EN 10131 normal tolerance. On the special tolerance the figure is 4 mm (0.157 in). The ISO standard for laser cut quality says plainly that it does not address flatness and sends the reader to the standards for the material.
So the only place a buyer finds a number for the shape of the sheet before it is cut is the product standard, and the table in it is read by thickness, by width and by strength class.
What a Flatness Tolerance Covers Before the First Cut
In the EN 10131 and EN 10051 tables, as ArcelorMittal prints them, flatness is a maximum deviation in millimeters, and the tables apply to sheet, not to coil. The extract does not describe the set-up used to measure it. Both product standards give a normal and a special set, and the special set is tighter.
ISO 9013 closes the loop from the other side. Its scope says flatness defects are not addressed as such in the document and that the references are to the current standards for the materials used. Dimensional classes in the same standard then assume a sheet in suitable condition: the standard says material grade and sheet temperature, set against machine temperature, have to suit the elongation or contraction that comes with relief of residual stress and with heat during cutting.
The flatness tables are therefore the first term in the error budget of a cut part, and they are the largest. For the sheet above the EN 10131 figure is 8 mm, while the class 1 dimensional limit for a 200 mm feature on 2 mm sheet is 0.25 mm. That flatness figure is about thirty times larger than the dimensional limit, and it belongs to a different stage of the work.
ISO 9013 does not set a flatness limit. The sheet’s shape before cutting is governed by the product standard for the steel, in a table read by thickness, width and strength.
The Flatness Table for Cold Rolled Steel Under 260 MPa
For uncoated and electrolytically coated cold rolled steel with a yield strength below 260 MPa, EN 10131 sets flatness by width and by thickness in three classes: under 0.7 mm, 0.7 mm up to 1.2 mm and 1.2 mm and over. Table 1 gives each cell as normal over special, in millimeters with inches in brackets.
| Width | Thickness under 0.7 mm | Thickness 0.7 up to 1.2 mm | Thickness 1.2 mm and over |
|---|---|---|---|
| under 600 mm | 7 (0.276) over 4 (0.157) | 6 (0.236) over 3 (0.118) | 5 (0.197) over 2 (0.079) |
| 600 to under 1,200 mm | 10 (0.394) over 5 (0.197) | 8 (0.315) over 4 (0.157) | 7 (0.276) over 3 (0.118) |
| 1,200 to under 1,500 mm | 12 (0.472) over 6 (0.236) | 10 (0.394) over 5 (0.197) | 8 (0.315) over 4 (0.157) |
| 1,500 mm and over | 17 (0.669) over 8 (0.315) | 15 (0.591) over 7 (0.276) | 13 (0.512) over 6 (0.236) |
Thinner sheet is allowed to be less flat, and wider sheet is allowed to be less flat. At 1,500 mm and wider, a sheet under 0.7 mm thick may be 17 mm off flat on the normal tolerance, which is more than twice the 7 mm of the narrowest class. The special column cuts each cell by roughly half, from 17 to 8 mm for the widest and thinnest sheet and from 5 to 2 mm for the narrowest and thickest.
Why the table loosens for thin sheet is not stated in the extract. A thin sheet has little bending stiffness, so it takes the shape of its own residual stresses and its own weight, and a table that tightened with thinness would be unattainable. That reading is an engineering inference and not a statement of the standard.
The extract also does not state the length over which the flatness is measured for EN 10131. Table 3 below gives it for hot rolled sheet, at 1,000 mm, and a buyer who needs a firm check method asks the mill which one applies.
How Strength Above 260 MPa Changes the Flatness Limit
The EN 10131 values grow with the strength class. For 260 to 340 MPa yield, the EN 10131 values in the ArcelorMittal tables are larger for the same thickness and width, and the table has no row for sheet narrower than 600 mm. Above 340 MPa yield the tables give no values at all: the flatness has to be specified at the time of enquiry and order.
| Width | Thickness under 0.7 mm | Thickness 0.7 up to 1.2 mm | Thickness 1.2 mm and over |
|---|---|---|---|
| 600 to under 1,200 mm | 13 (0.512) over 8 (0.315) | 10 (0.394) over 6 (0.236) | 8 (0.315) over 5 (0.197) |
| 1,200 to under 1,500 mm | 15 (0.591) over 9 (0.354) | 13 (0.512) over 8 (0.315) | 11 (0.433) over 6 (0.236) |
| 1,500 mm and over | 20 (0.787) over 12 (0.472) | 19 (0.748) over 10 (0.394) | 17 (0.669) over 9 (0.354) |
Against Table 1, the 1.2 mm and thicker column for 600 to 1,200 mm width goes from 7 to 8 mm normal and from 3 to 5 mm special. The special column loosens more than the normal one, so the ratio between them narrows with strength: for that cell, 3 over 7 becomes 5 over 8.
Steel at 340 MPa and above is where the tables stop. A drawing that calls for high-strength sheet and relies on flatness has nothing in the standard to point to unless the order states a limit. The buyer writes the number, and the mill agrees to it or declines.
- State a flatness value in millimeters and the measuring length for any steel at 340 MPa or more.
- Ask for the special column when the nest is large or the parts have long flat faces.
- Say whether the number is for sheet as delivered or for sheet after leveling.
Edge Waves and Short Waves on Sheet Edges
EN 10131 adds a rule for waves along the edge that a flatness number alone would not catch. For a sheet narrower than 1,500 mm, the height of an edge wave longer than 200 mm has to stay under 1 % of its length. On a sheet 1,500 mm or wider, the limit is 1.5 % of its length. Waves shorter than 200 mm are limited to a maximum height of 2 mm (0.079 in).
The percentage rule scales with the wave. A 500 mm long wave on a narrow sheet may be as high as 5 mm, and one on a sheet 1,500 mm wide or more as high as 7.5 mm. In the first case, a 1,000 mm wave is allowed 10 mm.
Edge waves can cause trouble on parts nested near the sheet edge, since those parts inherit the wave. A nest that keeps its parts away from the outer strip of the sheet avoids the worst of it. The standard does not say how wide that strip is, and the figure needs a trial on the actual coil.
Flatness of Hot Rolled Sheet and Plate
Thicker blanks are often cut from hot rolled stock, and EN 10051 gives its flatness limits in a table that names the measuring length: 1,000 mm. The table is split by width, by thickness and by steel category, with categories A, B and C together and category D, the higher strength steels with yield strength from 420 to 960 MPa, separate. For thin sheet in category D the values are to be agreed with the customer.
| Thickness | Normal, categories A to C | Normal, category D | Special, categories A to C | Special, category D |
|---|---|---|---|---|
| up to 2.00 mm | 18 (0.709) | to be agreed | 18 (0.709) | to be agreed |
| over 2.00 to 2.50 mm | 15 (0.591) | to be agreed | 14 (0.551) | to be agreed |
| over 2.50 to 3.00 mm | 15 (0.591) | to be agreed | 11 (0.433) | to be agreed |
| over 3.00 to 5.00 mm | 15 (0.591) | 18 (0.709) | 9 (0.354) | 12 (0.472) |
| over 5.00 to 8.00 mm | 13 (0.512) | 16 (0.630) | 8 (0.315) | 11 (0.433) |
| over 8.00 to 15.00 mm | 13 (0.512) | 16 (0.630) | 7 (0.276) | 10 (0.394) |
| over 15.00 to 25.00 mm | 13 (0.512) | 16 (0.630) | 7 (0.276) | 10 (0.394) |
Hot rolled sheet loosens as it thins, the same as cold rolled, and the special column has the larger effect on thick plate. From 5 mm upward the special tolerance falls to around half the normal one, from 13 down to 7 mm for categories A to C at 8 to 25 mm thick. The hot rolled and cold rolled tables cannot be compared cell by cell, because the hot rolled one states its 1,000 mm measuring length and the cold rolled one, in the extract, does not.
Hot rolled categories deserve a note. EN 10051 sorts steels by yield strength: category A up to 300 MPa, B from 300 to 360 MPa, C from 360 to 420 MPa and D from 420 to 960 MPa, with a further group above 960 MPa. Flatness for A, B and C shares one column, while category D has its own, because the stronger steel is harder to hold flat. That last clause is the maker’s table logic read as inference, since the document gives the columns and not the reason.
What Eight Millimeters Means Across a Sheet
Take the 8 mm figure and read it as one smooth bow across the 1,250 mm width of the sheet. The edges then tilt away from the chord by about 4 x 8 / 1,250 = 0.026, or roughly 1.5°, and a 200 mm part nested near an edge sits on a surface tilted by that amount. That is an illustration, since real sheets carry waves and twists and not a single bow, and the tables do not describe the shape of a deviation, only its largest value.
The illustration shows why a flatness table and a dimensional table do not compete. One describes the shape of the sheet before cutting, and the other describes the cut in the plane of the sheet. A part can meet its ISO 9013 class and still carry the sheet’s curvature into the bend, which the brake then has to deal with.
Flatness tells you how the sheet sits before the laser, not how well the laser cuts. A 4 mm special tolerance on a 1.5 mm sheet is a sheet condition to order, and the cutter cannot add it back afterward.
What These Flatness Tables Do Not Cover
The ArcelorMittal tables are the maker’s guarantees for its own steel products, and they stop at the steels they list. Hot dip coated sheet to EN 10143 has its own flatness table in the same document, which this piece does not reproduce because the extract merges cells in a way that cannot be read with confidence. A buyer of galvanized sheet reads that table in the source and not in a summary.
Stainless steel and aluminum are outside these tables. The stainless finish guide and the stainless bulletins opened for these resources give no flatness numbers, and the aluminum data sheets cite ASTM B209M, EN 485-2 and AS/NZS 1734 as the standards that govern the sheet without printing their flatness limits. For those materials the number comes from the product standard and the mill, and a drawing that wants flat stainless or aluminum sheet asks for it by name and value. A face that needs flatness beyond what the sheet delivers is not drawn from this table. It is left with stock on it and finished on a mill after cutting, which is where the tolerance becomes a machined steel face rather than a property of the coil.
What Flatness Does on the Laser Bed and the Brake
A sheet that is not flat affects the work downstream in at least one way the standards name. On the laser it can change the distance between the nozzle and the work, a distance ISO 9013 lists among the terms of the process in its first figure, without giving a tolerance for it. The effect on the brake is left to the shop’s own trial, since neither table addresses it.
Mills can improve the first stage. Euro Inox notes that the 2B stainless finish, cold rolled, heat treated, pickled and skin passed, is common for good corrosion resistance, smoothness and flatness, and that skin passing may be complemented by tension leveling. For large stainless panels, the same guide says pattern rolled sheet stiffens thin gauges and reduces oil canning, the visible distortion of large flat areas.
The cutting step can undo some of the gain. Residual stress inside a sheet is released as material is cut away, and ISO 9013 names this as a reason dimensional classes depend on material and temperature. A part cut from a stressed sheet can move after it leaves the skeleton, with the movement set by the layout of the nest and not by the nominal flatness of the sheet.
That leaves a question about nesting that no table answers, and a first article is the test.
Ordering Flat Sheet and Checking a Delivery
As with the thickness tables, the maker notes that the current standard prevails over its printed values, so a flatness requirement on an order cites the standard and its year and does not point at a brochure. An order for sheet that has to stay flat through cutting should name the product standard, the strength class, the width class and the column. For steel at 340 MPa and above, it should name a number in millimeters, since the standard leaves that to the order. A first run of cut parts at low-volume sheet metal gives the first measurement of how the sheet behaves on a particular laser and brake, and the nest layout that works becomes part of the record a later bridge production run repeats.
- Name EN 10131 or EN 10051 and the strength class on the order.
- State normal or special for flatness, since the two tables differ by about half.
- Give a number and a measuring length for steel at 340 MPa and above.
- Keep parts out of the edge strip, where the edge wave rule allows the largest height.
Sources and Further Reading
- ArcelorMittal Europe, Flat Products, Tolerance and conversion tables (EN 10051, EN 10131, flatness)
- ISO, ISO 9013:2017, Thermal cutting, Classification of thermal cuts, Geometrical product specification and quality tolerances (full text, UNE licensed copy held in a third-party document store)
- Euro Inox, Guide to Stainless Steel Finishes, Building Series Volume 1, third edition 2005