DrawingCut EdgeJoint

ISO 1461 Hot-Dip Galvanizing of Fabricated Steel Parts

ISO 1461 sets zinc thickness by steel thickness, measures it away from edges, and expects cut edges ground and parts bent before galvanizing.

Heavy hot-dip galvanized fabricated steel parts with a thick matte grey zinc coat, a welded bracket and a short frame section, one with a small drip of zinc at an edge.

A bracket cut from 2 mm (0.079 in) steel and hot-dip galvanized to ISO 1461 is owed a mean zinc coating of 55 µm (2.2 mil), and no reference area on it may average less than 45 µm (1.8 mil). The same standard then says that none of those measurements may be taken within 10 mm (0.39 in) of an edge, on a cut surface or on a corner, and its note on laser, plasma and flame cutting explains why: those edges are where the coating forms least reliably. On a small sheet metal part, a good share of the surface is exactly that zone.

ISO 1461, published in the UK as BS EN ISO 1461, is the standard the Galvanizers Association describes as the recognized specification for galvanizing after fabrication. It sets the coating thickness, the appearance, the repair rules and the sampling for acceptance, and it leaves several questions to the purchaser. For cut, bent and welded sheet parts those open questions matter more than they do for heavy structural steel, and the sections below read the standard with that kind of part in view.

What ISO 1461 Covers for Cut and Bent Steel Parts

ISO 1461:2022, the fourth edition, sets out the properties and test methods of zinc coatings formed when finished iron and steel articles, some castings included, are dipped in molten zinc holding at most 2 % of other metals. Its key word is fabricated: the parts are cut, formed and welded first and galvanized afterward in batches, by a company the standard now defines as the galvanizer.

The scope excludes three product groups. Sheet, wire and mesh galvanized continuously are outside it, as are tube and pipe galvanized in automatic plants and products such as fasteners with their own standards. Pre-galvanized coil, the material behind galvanized sheet designations, is therefore a different subject; ISO 1461 starts when a finished part goes into the kettle.

The fourth edition replaced ISO 1461:2009. Its foreword lists the main changes: added definitions, among them galvanizer, wet storage stain and duplex system; clarified rules for choosing reference areas, including avoiding small ancillary elements on a larger article; revised renovation rules; all coating thickness requirements gathered in clause 6.5 with Tables 3 and 4; recognition of the lower thicknesses that ultra-low reactive steels can give; and updated corrosion information referring to ISO 9224.

ISO 1461 is a standard for parts galvanized after fabrication. A drawing that calls it is asking for a dipped finished part, not for galvanized sheet.

What the Standard Leaves to the Steel

Clause 4.1 is frank about what it does not control. It accepts that the steel’s chemistry and surface, the weight of the parts and the bath conditions all influence how the coating looks, how thick it grows and how it behaves, and it places no requirement on any of them. For guidance it points to ISO 14713-2. The steel order, not the galvanizing order, is where those factors are fixed.

Coating Thickness by Steel Thickness

Minimum coating depends on the sheet thickness or section thickness underneath, because thicker sections react longer in the zinc. The UK trade body, the Galvanizers Association, prints the requirements for articles that are not centrifuged, which covers almost every sheet metal part.

Table 1. ISO 1461 minimum coating on articles not centrifuged, as printed by the Galvanizers Association
Article and steel thickness Local coating, minimum Mean coating, minimum
Steel over 6 mm (0.236 in) 505 g/m², 70 µm (2.8 mil) 610 g/m², 85 µm (3.3 mil)
Steel over 3 mm up to 6 mm (0.118 to 0.236 in) 395 g/m², 55 µm (2.2 mil) 505 g/m², 70 µm (2.8 mil)
Steel 1.5 mm up to 3 mm (0.059 to 0.118 in) 325 g/m², 45 µm (1.8 mil) 395 g/m², 55 µm (2.2 mil)
Steel under 1.5 mm (0.059 in) 250 g/m², 35 µm (1.4 mil) 325 g/m², 45 µm (1.8 mil)
Castings 6 mm (0.236 in) and over 505 g/m², 70 µm (2.8 mil) 575 g/m², 80 µm (3.1 mil)
Castings under 6 mm (0.236 in) 430 g/m², 60 µm (2.4 mil) 505 g/m², 70 µm (2.8 mil)

Mass and thickness are linked by the nominal zinc density the standard uses in disputes, 7.2 g/cm³: 325 g/m² over 7.2 g/cm³ gives the 45 µm in the table. Mil values are the writer’s conversions.

Most cut and bent sheet parts fall in the bottom two steel rows, and thin sheet under 1.5 mm in the last of them. A 1.2 mm cover and a 2 mm bracket on the same assembly therefore carry different minimums, 45 and 55 µm mean, and a drawing that names one coating thickness for the whole assembly has picked one row for parts that sit in two.

Why Thickness Is the Number That Matters

Clause 6.2.1 gives the reason the standard is built on thickness: the duration of corrosion protection from a galvanized coating is approximately proportional to its thickness, with ISO 14713-1 as the reference. The Galvanizers Association describes the coating as a series of hard zinc-iron alloy layers under an outer layer of soft pure zinc, which forms wherever zinc can reach, inside properly vented hollow sections and into recesses, edges and corners, and protecting exposed steel sacrificially where the coating is damaged. It adds that a magnetic gauge checks the thickness on site without harming the coating.

For a sheet part, that proportionality is the uncomfortable fact. A 1.2 mm part is owed 45 µm mean against 85 µm on structural steel over 6 mm, so in the same environment it is protected for a shorter time, and a design life that assumes the heavy-section coating on a light sheet part is assuming twice the zinc it will get.

Local and Mean, and How the American Standard Compares

ISO 1461 sets two numbers per row. The local thickness is the mean of the measurements inside one reference area; the mean thickness is the average of all local values. Its American counterpart, comparing ISO 1461 with ASTM A123, notes that the ISO local minimums sit 0.4 to 0.6 mil (10 to 15 µm) below the mean minimums, that the differences in minimum average thickness between the two standards are small for most steel, and that the ASTM specifications typically ask for somewhat more coating. It also notes that galvanizing to A123 will typically give a result that meets or exceeds ISO 1461, that ISO 1461 puts all its non-centrifuged requirements in one table with no coating grades, and that it brings centrifuged articles, covered in the US by ASTM A153, into the same standard.

The Galvanizers Association adds two practical points. Real coatings often exceed the minimum, and thicker coatings, where an aggressive environment calls for them, can come from grit blasting before galvanizing or from the steel’s own section and chemistry, to be agreed with the galvanizer before specification. In a small number of cases, it warns, unreactive low-silicon steels prevent the standard’s thicknesses from being reached, which is the case the 2022 edition now addresses for ultra-low reactive steels.

Steel Chemistry Before the Part Is Cut

Because the steel’s composition controls the zinc reaction, the right moment to settle galvanizing is the steel order. Mills mark which of their products suit it. ArcelorMittal’s structural steel page lists suitability for galvanizing as an option to be agreed, designated +CL1 or +CL3, and its chemistry table marks standard EN 10025-2 grades “No” and its own controlled versions Class 1 or Class 3. SSAB’s Domex 420MC data sheet states that its silicon of 0.03 % at most meets category A for thin hot-dip zinc coatings under EN 10149-2, with category B for thick coatings, at 0.15 to 0.21 % silicon, available on request.

  • Thin, even coating wanted: a steel declared suitable for galvanizing, such as a category A or Class 1 product.
  • Thicker coating wanted: a reactive steel or grit blasting, agreed with the galvanizer first, since the Galvanizers Association treats reactive steel as appropriate only for certain applications.
  • Mixed steels in one welded assembly: expect different coating thickness and appearance on each, since clause 4.1 ties both to the steel.

Appearance, Cut Edges and Venting

The appearance requirement is short and practical. At acceptance, the visible significant surfaces, examined by normal or corrected vision from not less than 1 m (3.3 ft), are to be free from blisters, from roughness and sharp points that can cause injury, and from uncoated areas. Darker or lighter areas such as a cellular pattern or dark grey, some unevenness such as orange peel, and weld seepage from intermittent welds round overlapping surfaces are not causes for rejection. Wet storage stain, the white zinc corrosion product that forms on fresh coatings stored damp, is not a cause either, provided the thickness stays above the minimum.

The standard is equally frank about aesthetics. Its primary purpose is corrosion protection, and where appearance matters, it highly recommends that galvanizer and purchaser agree beforehand on the finish achievable, adding that no definition of appearance can cover all requirements.

A galvanized sheet part is accepted on coverage and thickness. Anything about how it looks has to be agreed in writing before it is dipped.

Laser-Cut Edges Before Galvanizing

For sheet metal the most important line in the standard is a note in clause 6.2.3. Flame cutting, laser cutting and plasma cutting change the steel’s composition and structure on and around the cut surface, so the minimum coating can be harder to reach there and the coating can show decreased cohesion or adhesion. To get the required thickness more reliably and secure adhesion, the standard advises that such cut surfaces be ground off and sharp edges removed during fabrication, before delivery to the galvanizer, with a cross-reference to Annex A.2 and to ISO 14713-2.

That puts edge finishing on the fabricator’s side of the order. A laser-cut part sent to the galvanizer with its cut edges untouched can meet every measurable clause, since measurements skip the edges, and still carry a thin or poorly bonded coating exactly where corrosion starts on a sheet part.

Venting, Overlaps and Hollow Sections

Clause 4.4 requires venting and draining according to Annex B, the standard’s normative safety and process requirements. Its definition of weld seepage, pre-treatment solution escaping from narrow spaces between closely contacting surfaces joined by intermittent welds, or from pinholes in welds, describes what happens when overlaps are not designed for the bath. Clause 6.1 also accepts that flux residues and zinc ash cannot always be removed where access is restricted, for example inside hollow sections. A welded box or a lapped joint on a sheet assembly is designed for galvanizing before it is welded, not after.

Sampling, Reference Areas and Measurement

Acceptance inspection takes place at the galvanizer’s plant before the products leave its custody, unless the order says otherwise, and covers appearance and coating thickness. Adhesion is tested only by agreement. Where the purchaser asks for a thickness test, the control sample size follows Table 1 of the standard.

Table 2. ISO 1461 control sample size related to lot size, Table 1 of the standard
Articles in the inspection lot Minimum articles in the control sample
1 to 3 All
4 to 500 3
501 to 1,200 5
1,201 to 3,200 8
3,201 to 10,000 13
over 10,000 20

An inspection lot is a single order or a single delivery load. For very small articles the standard lets the sampling schemes of ISO 2859 Parts 1 to 3 be used instead.

Reference Areas on Small Parts

Each reference area is at least 10 cm² (1.55 in²), and the number per article depends on its significant surface: three or more above 2 m², one from 100 cm² to 2 m² and one from 10 to 100 cm². Articles of 10 cm² or less are grouped, N articles together making up one reference area, and the total tested is N times the Table 2 number for the lot. When more than five articles are needed to make up one area, a single magnetic reading is taken on each where a suitable surface exists, and otherwise the gravimetric test is used.

Within each reference area at least five magnetic readings are taken, and a single reading below the local minimum does not matter, because only the area’s average counts. On long articles, reference areas sit near the center and about 100 mm (3.9 in) from the edges and ends. No reading is taken on cut surfaces, within 10 mm of edges, on flame-cut surfaces or on corners, and, unless agreed otherwise, not on small ancillary elements such as stiffeners, end plates and brackets on a larger article.

The standard explains why single magnetic readings are not judged one by one. Each reading covers a very small area, so single values can fall below the local or mean thickness; with enough readings inside a reference area, the magnetic and gravimetric methods give effectively the same local thickness. A buyer checking a delivered part with a hand gauge therefore takes at least five readings per area and compares their average, never one low reading, with the table.

  • Routine method: magnetic gauges under ISO 2178 or ISO 2808, the most appropriate in works and for routine control.
  • Dispute method: gravimetric determination of mass per area under ISO 1460, converted at 7.2 g/cm³.
  • Protection for small lots: where fewer than 10 articles are involved, the purchaser need not accept a gravimetric test that destroys articles at unacceptable remedial cost.

Renovation, Adhesion and the Purchaser’s Information

Uncoated spots can be repaired, within limits. The galvanizer may renovate uncoated areas totaling no more than 0.5 % of the article’s surface, each no larger than 10 cm²; beyond that, the article is re-galvanized unless agreed otherwise. Repair is by zinc-rich paint with zinc dust or lamellar zinc pigment, a zinc paste or zinc alloy stick, or thermal zinc spraying, and the repair coating gives sacrificial protection. It averages at least 100 µm (3.9 mil) unless agreed otherwise, for instance where a different thickness suits the surrounding coating or a paint follows.

Clause 6.4 says no suitable International Standard exists for testing adhesion on fabricated articles, and that adhesion does not generally need testing, since good bonding is characteristic of the process. It adds a line every sheet metal buyer should read: bending or forming after galvanizing is not considered normal handling. A part is bent first and galvanized afterward.

Who Tells the Galvanizer

Often the galvanizer is not the buyer’s supplier at all. The Galvanizers Association explains that the galvanizer is normally the fabricator’s subcontractor and holds its contract with the fabricator, so the client’s galvanizing demands go into the fabricator’s specification, and the fabricator hands them on. It also points to the structural specifications that reference galvanizing, among them EN 1090-2 for the execution of steel structures. For a buyer of sheet parts, that chain means every galvanizing requirement, from the standard’s edition to the edge preparation and the paint plan, is written on the order to the fabricator, because nothing reaches the kettle any other way.

Clause 6.1 adds the consequence of a failed visual inspection: the articles are renovated within the limits above, or otherwise re-galvanized and resubmitted.

What the Purchaser Supplies

Under clause 4.3, the purchaser supplies the information listed in Annex A.1 and A.2, the standard’s normative list of what the galvanizer needs to know, and the 2022 edition points cut-edge preparation back to the same annex. Where the galvanized part will be painted, a sample is produced on request, and a purchaser can ask the galvanizer not to quench, not to apply an after-treatment, or to protect the parts from corrosion products in storage and transport. Those choices matter for a duplex system, which the standard now defines as a galvanized coating with an additional liquid paint or powder coating.

A batch of galvanized sheet parts goes smoothly when the drawing names ISO 1461:2022, the steel is ordered suitable for galvanizing, cut edges are ground and sharp edges removed before dipping, overlaps are vented, and the paint plan is told to the galvanizer up front. First lots of such parts suit low-volume sheet metal, and the thickness readings and appearance sample agreed on that lot are what a later bridge production run is accepted against.

How much thinner the coating on a ground laser edge runs than on the face of the same 2 mm part is a figure none of the documents cited here prints.

Sources and Further Reading

Request a Sheet Metal Quote

Send the 2D drawing and the 3D file, with the quantity and the stage of the project. An engineer replies within 1 working day.

The quote form, the mutual NDA and the private folder for your files are on Protolis Atelier, with Sheet Metal chosen.

Request a Quote