AluminumThin SheetCut Edge

ISO 9013 Laser Cut Edge Quality Ranges for Squareness and Roughness

Pick a squareness range and a roughness range by thickness, add the dimensional class, and agree how thin sheet is measured.

The laser cut edges of thick mild steel and stainless steel plates, fine vertical striations on the cut faces.

A laser cut in 2 mm sheet earns ISO 9013 squareness range 1 when its edge leans less than 0.056 mm (0.0022 in) from true over the full thickness of the sheet. The standard’s own coarse measuring instruments, a workshop square and feeler gauges, carry an error limit of 0.1 mm (0.004 in). So the tool the standard allows for the quick check is blunter than the tightest number it asks the check to resolve, and the precision tier it lists, a dial gauge on a guide, is good to 0.02 mm (0.0008 in).

That gap between a printed range and the way it is measured is the practical content of ISO 9013. The standard classifies thermal cuts by two edge values and one size class, and every one of the three has conditions attached.

What the ISO 9013 Ranges Tell You About a Laser Cut Edge

ISO 9013:2017 presents geometrical product specifications and quality tolerances for thermal cuts in materials suitable for oxyfuel flame cutting, plasma cutting and laser cutting. Its scope runs from 3 mm to 300 mm for flame cuts, 0.5 mm to 150 mm for plasma cuts and 0.5 mm to 32 mm for laser cuts. The standard applies only when a drawing or a delivery document refers to it. This third edition, dated February 2017, replaces the 2002 edition and was technically revised.

Two characteristic values describe a cut face. The perpendicularity or angularity tolerance u is the distance between two parallel lines that enclose the cut face profile at the set angle, 90° for a vertical cut. It captures squareness and flatness of the face together. The mean height of the profile Rz5 is the arithmetic mean of five consecutive single profile elements, and it describes roughness.

Each value has numbered ranges, with 1 the finest. The standard gives five ranges for u and four for Rz5, and each range is a formula of the cut thickness a. A third item, the dimensional class, is a separate choice and takes the value 1 or 2.

ISO 9013 describes a cut edge with two measured values, squareness u and roughness Rz5, each in numbered ranges that grow with sheet thickness. The size of the part is a third, separate choice.

Squareness Ranges 1 to 5 by Sheet Thickness

The ranges for u come from Table 4 of the standard. In millimeters, range 1 is 0.05 + 0.003 a, range 2 is 0.15 + 0.007 a, range 3 is 0.4 + 0.01 a, range 4 is 0.8 + 0.02 a and range 5 is 1.2 + 0.035 a, where a is the cut thickness in millimeters. Table 1 evaluates the formulas at thicknesses a laser shop sees.

Table 1. Perpendicularity or angularity tolerance u by range and thickness, in mm (in), evaluated from ISO 9013:2017 Table 4
Thickness a Range 1 Range 2 Range 3 Range 4 Range 5
1 mm (0.039 in) 0.053 (0.0021) 0.157 (0.0062) 0.410 (0.0161) 0.820 (0.0323) 1.235 (0.0486)
2 mm (0.079 in) 0.056 (0.0022) 0.164 (0.0065) 0.420 (0.0165) 0.840 (0.0331) 1.270 (0.0500)
3 mm (0.118 in) 0.059 (0.0023) 0.171 (0.0067) 0.430 (0.0169) 0.860 (0.0339) 1.305 (0.0514)
6 mm (0.236 in) 0.068 (0.0027) 0.192 (0.0076) 0.460 (0.0181) 0.920 (0.0362) 1.410 (0.0555)
10 mm (0.394 in) 0.080 (0.0031) 0.220 (0.0087) 0.500 (0.0197) 1.000 (0.0394) 1.550 (0.0610)
20 mm (0.787 in) 0.110 (0.0043) 0.290 (0.0114) 0.600 (0.0236) 1.200 (0.0472) 1.900 (0.0748)

Two features of the table matter for sheet. First, the constant term dominates in thin material: the formula for range 3 gives 0.41 mm at 1 mm and 0.50 mm at 10 mm, so a tenfold increase in thickness adds only 0.09 mm to the allowance. Second, the ranges are spaced by a factor of about three at the bottom, from 0.056 mm to 0.164 mm at 2 mm, and the jump from range 1 to range 2 is the one that decides whether a precision gauge is needed to prove the cut.

Perpendicularity is not the same as lean alone. The standard says u includes flatness deviations of the cut face, so a face that bows by a few hundredths of a millimeter and a face that leans by the same amount both use up the allowance.

Roughness Ranges 1 to 4 by Sheet Thickness

Table 5 of the standard sets Rz5 in micrometers: range 1 is 10 + 0.6 a, range 2 is 40 + 0.8 a, range 3 is 70 + 1.2 a and range 4 is 110 + 1.8 a, with a in millimeters. Table 2 evaluates them, with the value in microinches beside it.

Table 2. Mean height of the profile Rz5 by range and thickness, in µm (µin), evaluated from ISO 9013:2017 Table 5
Thickness a Range 1 Range 2 Range 3 Range 4
1 mm (0.039 in) 10.6 (417) 40.8 (1,606) 71.2 (2,803) 111.8 (4,402)
2 mm (0.079 in) 11.2 (441) 41.6 (1,638) 72.4 (2,850) 113.6 (4,472)
3 mm (0.118 in) 11.8 (465) 42.4 (1,669) 73.6 (2,898) 115.4 (4,543)
6 mm (0.236 in) 13.6 (535) 44.8 (1,764) 77.2 (3,039) 120.8 (4,756)
10 mm (0.394 in) 16.0 (630) 48.0 (1,890) 82.0 (3,228) 128.0 (5,039)
20 mm (0.787 in) 22.0 (866) 56.0 (2,205) 94.0 (3,701) 146.0 (5,748)

Range 4 is ten times as rough as range 1 at 2 mm. Rz5 is a peak-to-valley measure and runs larger than the average roughness Ra that most drawings quote, so a callout of Ra 3.2 µm cannot be read against this table directly.

The standard states Rz5 is measured at one place and with one method, and the next section gives them.

How and Where the Edge Is Measured

ISO 9013 puts the measuring rules in clause 6, and they decide what a stated range means in practice. The measurements are made on brushed cuts that are free from oxides, outside areas that contain imperfections, with the upper and lower sheet faces as reference. Piercing areas, the start of the cut and its end are excluded. If a drawing does not specify a count, the standard defines one: for u, two series of three measurements 20 mm apart on each meter of cut, and for Rz5, one measurement on each meter.

The measured zone is smaller than the face. Upper and lower edges are excluded by a distance Δa, set in Table 3 of the standard, to allow for the melting of the top edge.

Table 3. Edge zone excluded from the u measurement, by cut thickness (ISO 9013:2017 Table 3)
Cut thickness a Δa taken off the upper and the lower edge
up to 3 mm (0.118 in) 0.1 a
over 3 mm up to 6 mm (0.236 in) 0.3 mm (0.012 in)
over 6 mm up to 10 mm (0.394 in) 0.6 mm (0.024 in)
over 10 mm up to 20 mm (0.787 in) 1 mm (0.039 in)
over 20 mm up to 40 mm (1.575 in) 1.5 mm (0.059 in)

For a 2 mm sheet, Δa is 0.2 mm at each edge, so u is read on 1.6 mm of the 2 mm face. Roughness is read at 15 mm from the start of the cut in the advancing direction, at the point of greatest roughness, per ISO 4288 with an instrument as in ISO 3274. For a sheet thinner than 2 mm the standard moves the Rz5 measurement to half the cut thickness below the upper edge.

The standard sets two instrument tiers. Precision instruments carry error limits of 0.02 mm for u and 0.002 mm for Rz5, with a dial gauge guided along the face for the former and an electric contact stylus for the latter. Coarse instruments, such as a workshop square, depth gauge or feeler gauge, carry 0.1 mm for u, and the standard lists no coarse method for Rz5.

If readings land near the lower limit of a range, extra measurements are advised. Near the upper limit, or with a result in doubt, the standard requires supplementary measurements at the same number of additional points.

  • A range 1 or range 2 callout on thin sheet makes the coarse tier’s 0.1 mm error a large share of the limit, 61 % of range 2 at 2 mm.
  • A cut under 2 mm thick has no standard method for u, because the standard says the procedure has to be agreed.
  • Dross or melted drops at the lower edge are listed by the standard as additional characteristics, apart from the two ranges.

Writing the Designation on a Drawing

A cut that meets the standard is designated by the words thermal cut, the number of the document, the range for u, the range for Rz5 and the dimensional class. The example in the standard is ISO 9013-312:2017, with u in range 3, Rz5 in range 1 and tolerance class 2. On a drawing the same information is given in a surface texture symbol, with the u range, then the Rz5 range, then the class, and in a title block it is written as ISO 9013-342 for u range 3, Rz5 range 4 and class 2.

The order, u first and Rz5 second, is fixed, and where no value is set for one of them a zero takes its place. A designation such as ISO 9013-302 therefore says nothing about roughness, and a designation such as ISO 9013-012 says nothing about squareness.

Writing only “ISO 9013” on a drawing has not chosen a range. The ranges are a menu and the standard does not rank them as a default. A drawing that writes “range 3” without a document edition leaves open which revision’s formulas apply, and the 2017 text is a technical revision of the 2002 one.

The count rule has a practical meaning for a long cut. A 3 m run of cut length, measured under the default rule, yields six readings of u in two series of three on each meter, which is 18 in all, and three readings of Rz5. Cuts under a meter long carry a single set. The standard lets the manufacturer define the number and location of points, and says they belong where the largest values are expected, so the count is a floor for a report and not a sampling plan for an audit.

Annex B explains the three kinds of laser cutting the standard recognizes. In laser oxyfuel cutting the beam heats the material while an oxygen jet burns it. Fusion cutting melts the material with the beam and blows the melt away with a jet.

Sublimation cutting evaporates the material in the cut area. The annex notes that the achievable quality differs with the laser source, CO₂ or solid state, and the cut quality ranges describe the result and not the mechanism that produced it.

Two Example Callouts Worked Through

Take a 1.5 mm sheet bracket drawn as ISO 9013-222. Range 2 for squareness gives 0.15 + 0.007 x 1.5, which is 0.1605 mm (0.0063 in). Roughness in range 2 gives 40 + 0.8 x 1.5, which is 41.2 µm (1,622 µin).

Class 2 sets the size limits that the dimensional tolerance article reads in full. Since the sheet is under 2 mm, the method for u is left to agreement and Rz5 is read at 0.75 mm below the upper edge.

Now a 12 mm plate drawn as ISO 9013-342. Range 3 for squareness gives 0.4 + 0.01 x 12, which is 0.52 mm (0.0205 in). Roughness in range 4 gives 110 + 1.8 x 12, which is 131.6 µm (5,181 µin). Here Δa is 1 mm at each edge, so u is read on 10 mm of the 12 mm face, and the coarse instrument tier with its 0.1 mm error is about a fifth of the allowance.

The same formulas that give 0.16 mm of squareness on a thin bracket give 0.52 mm on a 12 mm plate, so a plate is not a bigger bracket. Pick ranges by thickness, and read them in millimeters, not as a grade.

What Annex A Says About Laser, Aluminum and Thin Sheet

Annex A is informative, and it holds three points a buyer of laser-cut sheet should know. The first is that laser cutting up to 32 mm typically achieves dimensional class 1, while oxyfuel flame and plasma cutting typically achieve class 2. Second, the annex states that the classes cannot be reached at the start and end of a cut, at small radii or at sharp angles for u and Rz5, and that they need serviced machines and trained operators.

Third come aluminum, titanium, magnesium and copper alloys. On these cuts, says the annex, a rippled surface appears, depending on the alloy’s grain structure, that Rz5 cannot be determined on it and evaluated by the standard, and that values about four times as high as the standard’s may be expected for aluminum and its alloys. A drawing that calls out an Rz5 range on an aluminum part is asking for something the standard says it cannot assess.

The annex also notes that the achievable level depends on the laser source, CO₂ or solid state, and that specialized laser cutting processes can give significantly lower Rz5 values. It gives no numbers for either. The ranges therefore describe what can be called out, and the capability of a particular machine and gas setup is found by sample cuts, a point that belongs to the cutting step and not to the standard.

What ISO 9013 Leaves to the Contract

Several things a drawing might assume are outside the document. Flatness defects of the sheet are not addressed, and the standard sends the reader to the material standards, which is the subject of the flatness tolerances on rolled sheet. Straightness, parallelism and perpendicularity of the whole cut, shown in its Figure 11 as tolerances referenced to ISO 1101, are not included in the ranges and need a separate agreement if they matter.

Four items sit outside the ranges.

  • Sheet flatness, which the standard hands to the material standards.
  • Straightness, parallelism and perpendicularity of the whole cut, which need their own agreement.
  • The measuring method for u on sheet under 2 mm.
  • The start and end of a cut, small radii and sharp angles, where the ranges do not apply.

Dimensional limits are also conditional for lasers. The standard says that the dimensional tolerances a laser can hold depend essentially on the length-to-width ratio of the part, its geometry and the pre-treatment of the sheet, and that the sheet temperature compared with the machine temperature has to suit the elongation or contraction of the material as stress relaxes. Limit deviations are treated apart from squareness because they have different causes.

Combined technologies, such as laser cutting followed by punching, are outside the typical classes in Annex A and have to be considered separately, because they bring application-specific tolerances of their own. Where a cut edge is finished afterwards, the standard’s clause 8 adds the squareness tolerance and the lower limit deviation to the allowance on outside dimensions, and it supplies a default machining allowance of 2 mm per cut surface for sheet from 2 to 20 mm thick when the drawing gives none.

A drawing that works with the standard names the ranges for the two edge values, the class for size, the edition, the measuring tier for the finest ranges, and the thin-sheet method if the sheet is under 2 mm. First runs of cut parts at low-volume sheet metal can then be checked against the same text that later bridge production runs use, with no argument about what range 2 meant.

Sources and Further Reading

Request a Sheet Metal Quote

Send the 2D drawing and the 3D file, with the quantity and the stage of the project. An engineer replies within 1 working day.

The quote form, the mutual NDA and the private folder for your files are on Protolis Atelier, with Sheet Metal chosen.

Request a Quote