A square meter of 2 mm 5052 sheet weighs about 5.4 kg (11.8 lb), taking the nominal density of 2.68 g/cm³ (0.097 lb/in³) that the Aluminum Association lists for the alloy. The same area in 316L stainless steel, at the 8.03 g/cm³ Cleveland-Cliffs prints, weighs 16.1 kg (35.4 lb). Two thirds of the weight disappears for the same thickness, and that is why 5052 shows up in enclosures, brackets, panels and tanks long before anyone argues about its strength.
The alloy then asks three questions of a drawing: which temper and which specification, how tight a bend the sheet will take, and what a weld does to the strength the temper gave it. The sections below take them in that order, from the alloy registration, the bending columns of The Fabricator and the filler guides of two welding consumable makers.
What 5052 H32 Offers a Bent and Welded Aluminum Part
Alloy 5052 is an aluminum-magnesium alloy, registered in the United States in 1954. The Aluminum Association’s international alloy register sets its composition: silicon 0.25 % maximum, iron 0.40 %, copper 0.10 %, manganese 0.10 %, magnesium 2.2 to 2.8 %, chromium 0.15 to 0.35 %, zinc 0.10 %, and 0.05 % each and 0.15 % in total for other elements, with aluminum the remainder.
That places it in the 5xxx series, the aluminum-magnesium alloys. A bending column in The Fabricator sets out why the series behaves as it does: alloys of the 1xxx, 3xxx, 4xxx and 5xxx series are not heat-treatable, because of the alloying elements they carry, while added copper, magnesium-silicon and zinc make the 2xxx, 6xxx and 7xxx series heat-treatable. A 5052 sheet therefore takes its strength from cold work, and the temper code records how much. H32 is strain-hardened and stabilized to a quarter-hard level, with H34, H36 and H38 harder in steps and O the soft annealed state.
For a cut, bent and welded sheet part, the temper is the real choice. H32 is stiff enough to hold a flat panel and soft enough to form, while the harder tempers give up bendability for strength, as the bending section below shows.
5052 H32 is a non-heat-treatable, quarter-hard aluminum sheet with magnesium as its main alloying element. Its strength comes from cold work, and the heat of a weld takes that work back out.
Stock sizes make the weight concrete. A 2,500 by 1,250 mm (98 by 49 in) sheet has an area of 3.125 m². At 2.68 g/cm³, a 1.5 mm sheet of that size weighs about 12.6 kg (27.7 lb) and a 3.0 mm sheet about 25.1 kg (55.4 lb). A part nested in it carries the mass in proportion to its area, so a bracket of 0.05 m² in 2 mm material is about 0.27 kg (0.59 lb) before any holes. A thicker part with pockets or bosses leaves the sheet alloys behind, since 6061 plate and bar are what machined aluminum parts are usually cut from, while 5052 stays the choice where the part is bent and welded from flat sheet.
Composition Against the Alloys It Is Confused With
Two neighbors in the register explain most of the substitutions a buyer meets. Alloy 5251, registered by the European Aluminium Association in 1972, carries less magnesium, 1.7 to 2.4 %, and allows more silicon, iron and manganese. Alloy 5754, registered in 1970, carries more, 2.6 to 3.6 %, with a combined manganese and chromium limit of 0.10 to 0.6 %. Their nominal densities sit within a few hundredths of 5052’s.
| Element or property | 5052 | 5251 | 5754 |
|---|---|---|---|
| Magnesium | 2.2 to 2.8 | 1.7 to 2.4 | 2.6 to 3.6 |
| Chromium | 0.15 to 0.35 | 0.15 | 0.30 |
| Manganese | 0.10 | 0.10 to 0.50 | 0.50 |
| Silicon | 0.25 | 0.40 | 0.40 |
| Iron | 0.40 | 0.50 | 0.40 |
| Copper | 0.10 | 0.15 | 0.10 |
| Zinc | 0.10 | 0.15 | 0.20 |
| Nominal density, g/cm³ (lb/in³) | 2.68 (0.097) | 2.69 (0.097) | 2.67 (0.097) |
The register prints a composition, not a strength. Mechanical properties belong to the product specification that governs the order, such as ASTM B209 in North America or EN 485-2 in Europe, and both set their values by temper and thickness. A drawing that says only “5052 H32” leaves the guaranteed figures to whichever specification the supplier happens to work to. A drawing that names the specification closes that question, and the mill certificate then reports the tested values of the actual lot.
The same reasoning covers substitution. An order for 5052 that is filled with 5251 or 5754 is filled with a different alloy, with a different magnesium content and different guaranteed properties, even where the two look alike on the shelf. If a substitute is acceptable, the drawing or the order says so.
Strength by Temper and What the Bending Columns Use
Strength rises with each step of cold work. The Fabricator’s column on predicting an air-formed bend radius works with tensile strengths of 33,000 psi (228 MPa) for 5052-H32, 38,000 psi (262 MPa) for H34, 40,000 psi (276 MPa) for H36 and 42,000 psi (290 MPa) for H38, values it takes from a materials database rather than from a specification. They serve its calculation and show the trend: the step from H32 to H38 adds about a quarter to the tensile strength.
The same publication’s column on formable aluminum reads formability as elongation and as the gap between yield strength and tensile strength. In the annealed temper, it gives 5052 an elongation of 20 % and a difference of 21.5 ksi (148 MPa) between yield and tensile strength, and it ranks the alloy a close second in formability among the alloys it compares. The column adds that aluminum work-hardens as it is formed, getting stronger and harder as it is bent, which is the same mechanism the H tempers are made by.
| Temper | Tensile strength, MPa (psi) | Change from H32 |
|---|---|---|
| H32 | 228 (33,000) | none |
| H34 | 262 (38,000) | +15 % |
| H36 | 276 (40,000) | +21 % |
| H38 | 290 (42,000) | +27 % |
For a buyer the table is a guide to direction, not a source of design values. The guaranteed minimums of the governing specification and the tested values on the mill certificate are what a calculation of a load-bearing part rests on.
Minimum Bend Radius for 5052 H32 Sheet
Bending is where the temper shows first. The Fabricator’s column defines the minimum bend radius as the point at which cracks start to appear on the outside surface of the bend, where the grains of the material begin to separate. As the inside radius shrinks relative to the thickness, the tensile strain on the outside surface grows.
The column gives a way to estimate that limit from a tensile test. It takes the tensile reduction of area, r, the percentage by which the cross section of a tensile specimen shrinks at the point of fracture, and gives the minimum inside radius as the thickness times (50 / r − 1). A material with a reduction of area of 25 % gives a minimum radius of one thickness, and one with 50 % gives zero, a bend that closes flat without cracking. The figure for a given lot comes from its own tensile test or from reference data.
Published charts give the same answer in a simpler form. The column’s chart shows a minimum inside radius of 0 to 1 times the thickness for 0.125 in (3.2 mm) 5052-H32, and it prints that figure next to a reader’s note that a supplier suggested at least 1.5 times the thickness for the same sheet. The column’s own advice is that fabricators check the recommended minimum radius with their material supplier, and the two figures together show why: at 3.2 mm, the difference between 1 t and 1.5 t is 3.2 against 4.8 mm (0.13 against 0.19 in) of inside radius.
| Multiple of thickness | Inside radius, mm (in) | Where the figure comes from |
|---|---|---|
| 0 t | 0 | lower end of the column’s chart |
| 1 t | 3.2 (0.125) | upper end of the column’s chart |
| 1.5 t | 4.8 (0.19) | the supplier’s suggestion quoted in the column |
The direction of the bend relative to the rolling direction is the other variable, and it is not printed in either figure. A drawing whose radius sits close to the published minimum therefore states the bend direction, and a trial bend in the real thickness and direction is the check that closes the gap.
- Write the inside radius as a number, not as “tight,” since a punch nose has a fixed radius.
- Draw radii above the minimum in the governing specification or the supplier’s table, and note the direction where the margin is small.
- Keep holes and slots clear of the bend line, because a distorted hole is the first visible sign of a bend that was too tight.
The Radius an Air Bend Actually Forms
The minimum is a limit. In air bending on a press brake, the radius the sheet takes is set by the die opening, and The Fabricator’s columns give two ways to estimate it.
The first is the rule its author calls the 20 percent rule, named after stainless steel, which forms an inside radius of about 20 to 22 % of the die opening. Softer materials form less. In its column on formable aluminum the author gives 11 to 13 % of the die opening for 5052 H32, against 15 to 17 % for 60 ksi cold-rolled steel and 18 to 20 % for 6061 in the O condition.
The second is a formula scaled from a baseline of 60,000 psi mild steel: inside radius equals the part’s tensile strength over the baseline’s, times the die width, times 0.1. For the 33,000 psi 5052-H32 of the reader’s question it gives 0.034 in (0.88 mm) over a 16 mm (0.630 in) die, and the column reports that it reproduced the reader’s measured 0.109 in (2.77 mm) over a 50 mm die. The two methods do not agree for the 16 mm die, and the author says plainly that the rule of thumb is a little imprecise and that a test bend, measured, gives the multiplier to use.
The column also warns about the punch. If the punch nose radius is much smaller than the radius the sheet floats to, the punch creases the center of the bend while the rest still floats a radius, and the bend turns from a curve into a sharp fold. For 5052 H32 that is the same crack risk as a radius below the minimum, reached another way.
In air bending, the die opening sets the radius 5052 H32 forms and a punch sharper than that radius creases the bend. A test bend in the shop’s own tooling turns both estimates into a number.
Laser Cutting 5052 Sheet
ISO 9013 is the standard most drawings name for a thermal cut edge. Its scope, as the Estonian standards body publishes it, covers materials suitable for oxyfuel flame, plasma and laser cutting, and applies to laser cuts from 0.5 to 32 mm, so a 5052 sheet from 0.8 to 6 mm sits inside it. The scope also says the geometrical specifications apply only where a drawing or a delivery condition refers to the standard, and that flatness defects are not addressed.
The standard’s quality ranges are a paid document, and their values are not printed here. What the scope does make clear is how the callout works: a drawing that names ISO 9013 and a range for squareness and roughness turns the edge into an inspected feature, and a drawing that names nothing leaves the edge to the cutter’s practice. On aluminum, whose cut faces differ in look from those of steel, a sample edge agreed with the cutter before the run is the practical reference.
Welding 5052 H32 Sheet, Filler and Heat
The filler is the first decision. ESAB notes that alloys with 1 to 2.5 % magnesium, 5052 among them, are very sensitive to cracking when they are welded with a filler of their own composition, and that a 5 % magnesium filler such as 5356 raises the magnesium in the diluted weld metal and lowers that sensitivity. Lincoln Electric gives 4043, 5554 or 5356 for 5052, with 5356 and 5554 used more often so that one filler serves the shop, and it notes that 4043 suits no other 5xxx alloy, because 5052 alone has that low a magnesium content. Lincoln notes that virtually all alloys of the 1xxx, 3xxx, 4xxx, 5xxx and 6xxx families are arc weldable by either TIG (GTAW) or MIG (GMAW), that preheat is rarely necessary with the correct equipment, and that argon shielding gas should flow at no less than 35 SCFH (16.5 L/min) for MIG and 25 SCFH (11.8 L/min) for TIG. It also asks that heavy oxides be removed before welding, with a sanding or grinding disk where material stored outdoors has built a heavy gray oxide.
The heat is the second. ESAB’s filler guide explains what a weld does to a non-heat-treatable alloy: the H temper produced by cold rolling is changed by the heat of welding to the annealed, O condition in the area next to the weld, since these alloys anneal at 600 to 700 °F (316 to 371 °C). In a groove weld, the annealed heat-affected zone is typically the weakest part of the joint, the welding procedure has little effect on the transverse tensile strength, and procedure qualification for these alloys is based on the minimum tensile strength of the base alloy in its annealed condition.
That changes the arithmetic of a welded 5052 H32 part. The strength the temper paid for is still there away from the seam, but the joint is designed to the annealed strength. A load-bearing bracket welded from H32 sheet is therefore sized as if the metal at the weld were soft, because it is.
Fillet welds follow a different rule. ESAB states that fillet weld strength depends largely on the composition of the filler and is rated in shear, that 4xxx fillers have lower ductility and give less shear strength in fillet-welded joints, and that in one test on 6061 a 1/4 in fillet with 5556 filler met the same shear requirement as a 7/16 in fillet with 4043. For a 5052 enclosure joined by fillets, the filler choice therefore sets the size of the weld.
Four points are worth settling before the first seam, and each is a line on the drawing.
- The filler, 5356 or 5554, or 4043 where the joint allows it, named for the alloy pair.
- An aluminum weld quality standard and level.
- The design strength at the weld, taken as annealed.
- A distortion allowance for long seams, since aluminum moves with the heat.
ISO 5817, the weld quality standard used on steel parts, does not apply. Its scope, as published, covers fusion-welded joints in steel, nickel, titanium and their alloys, and aluminum is not among them. A welded 5052 part takes its quality level from an aluminum weld standard, and a drawing that cites ISO 5817 level C on an aluminum seam has cited a document that does not cover the material.
Finishing 5052 Parts With Pretreatment and Coating
Aluminum sheet parts often go to powder coat. An IGP Powder Coatings data sheet for a matte powder lists the pretreatments it recommends for aluminum: chromating to DIN EN 12487, pre-anodizing, or a chrome-free pretreatment to GSB International and QUALICOAT specifications. It names a minimum test for aluminum and galvanized substrates, a boiling water test followed by a cross-cut adhesion and tape test, and it recommends a film thickness of 60 to 80 µm (0.0024 to 0.0031 in).
The data sheet leaves the choice of pretreatment to the coater to confirm with its own tests. A coating note on the drawing therefore names the powder system and the pretreatment standard, and asks for the adhesion test result on the first lot.
Reading a 5052 H32 Order
Because the register gives a composition and the specification gives the strength, the order is the document that fixes the material. Table 4 lists what to state and where each choice is defined.
| Item | What to state | Where it is defined |
|---|---|---|
| Alloy and temper | 5052 H32, substitutes named if allowed | Aluminum Association register |
| Governing specification | ASTM B209 or EN 485-2, named | the product specification |
| Mill certificate | tested values of the lot | the specification named |
| Inside bend radius | a number above the minimum, with direction where close | supplier’s table, trial bend |
| Laser edge | ISO 9013 and its ranges, or an agreed sample | ISO 9013 scope |
| Weld filler and standard | 5356, 5554 or 4043 by the joint, with an aluminum weld standard | ESAB, Lincoln Electric |
| Weld design strength | annealed strength at the joint | ESAB filler guide |
| Coating | pretreatment standard, film thickness, adhesion test | IGP data sheet |
In thin gauge, cut, bent and welded 5052 H32 is one of the easier jobs in sheet metal, and most of its trouble starts in the documents. First runs of such parts suit low-volume sheet metal, and a run that has settled into repeat orders is the moment to plan bridge production with the radius, the filler and the specification already fixed.
Sources and Further Reading
- International Alloy Designations and Chemical Composition Limits for Wrought Aluminum and Wrought Aluminum Alloys, revised August 2018, The Aluminum Association
- Predicting an Air-Formed Sheet Metal Inside Bend Radius, The Fabricator
- Formable Aluminum: Press Brake Bending 6061 With the 20% Rule, The Fabricator
- Selecting the Right Filler Alloy for Aluminum Welding, ESAB
- 6 Key Factors to Choose the Right Aluminum Filler Metal, ESAB
- Welding Aluminum in the Trailer Industry, Lincoln Electric
- 316 / 316L Stainless Steel Product Data Bulletin, May 2021, Cleveland-Cliffs
- ISO 9013:2017, Thermal Cutting, Classification of Thermal Cuts, scope page, EVS (Estonian Centre for Standardisation)
- ISO 5817:2023, Welding, Fusion-Welded Joints in Steel, Nickel, Titanium and Their Alloys, scope page, EVS (Estonian Centre for Standardisation)
- Technical Data Sheet IGP-DURA mix 3303E-A1, version 1.2, 24 April 2024, IGP Powder Coatings