A resistance spot weld on steel sheet runs at 8 to 15 kA for about one fifth of a second, according to the AHSS Insights guide on spot welding. A fusion seam on the same sheet keeps a torch moving along the joint for seconds per hundred millimeters, and the heat has that long to spread into the panel. The first joint is finished before the sheet notices. A seam leaves metal that shrinks as it cools and drags the panel with it.
Sheet metal assemblies are welded in both ways, often on the same part, and the order in which the joints are made decides whether the finished box is square. The sections below follow a welded sheet assembly from fit-up to inspection, using the distortion guidance of TWI, the stainless and aluminum producers’ own weldability notes, and the published spot welding practice.
Why Welded Sheet Distorts and in Which Directions
Weld metal shrinks as it solidifies and cools, and the cold sheet around it resists. The panel gives, and the way it gives depends on where the weld sits. TWI names three modes: angular distortion, a rotation of the plates about the seam, measured in degrees and affected by joint geometry, weld size and the number of runs; longitudinal shrinkage along the seam, which bows and buckles thin plate; and transverse shrinkage across the joint, which pulls the two sides together.
Thin sheet suffers most because it has little stiffness to push back. A 1.5 mm (0.059 in) panel has little stiffness along its unsupported edge, and a plate of 10 mm (0.39 in) has far more.
Stainless adds a material effect. Euroinox, in its guide to stainless steel finishes, points to the higher thermal expansion and lower thermal conductivity of stainless compared with carbon steel and says both should be accounted for in fabrication to minimize distortion. Heat stays near the seam and the expansion is larger, so the same procedure moves a stainless panel further than a mild steel one.
Distortion comes from the weld cooling against a panel that has no stiffness to resist it. Thin stainless shows it first.
Fit-up and Tack Welds Before Any Seam
Most distortion is settled before the first seam. TWI states that assembly technique often counts for more than welding procedure, and its guidance starts with tacks. Tacks set and hold the joint gap and resist transverse shrinkage. Too few of them, and the joint progressively closes up as welding proceeds, so the gap at the end of the seam is not the gap at the start.
| Technique | What it does | Mode it controls |
|---|---|---|
| Tack the full length, then weld | Holds the gap; plates are clamped or wedged | Transverse shrinkage |
| Tack one end, then back-step | Starts at a fixed end and works toward the free one | Transverse shrinkage and closing gap |
| Tack the center, then back-step | Starts mid-joint so both halves shrink toward a fixed point | Transverse shrinkage on long joints |
| Directional tacking | Closes a gap that is too wide | Gap that opens in fit-up |
| Back-to-back assembly | Two identical parts clamped together and welded in balance about the neutral axis | Angular distortion |
| Stiffening flats or angles | Longitudinal members welded along each side of a thin-plate seam | Longitudinal bowing |
TWI notes that back-to-back assemblies should be stress relieved before they are separated; without that step, wedges may be needed so the parts return to shape. A stiffener has to sit far enough from the joint not to interfere with welding, unless it is on the reverse side of a single-sided weld.
For sheet metal fabrications the common form is the tab-and-slot part: a laser cut panel with tabs that fit slots in its neighbor, which locates the parts and acts as a row of built-in tacks. The fit of those tabs, in turn, depends on the laser cut and the bend that came before, and an assembly that goes together by hand and stays square is far easier to weld than one clamped into position.
Back-Step and Skip Welding Sequences
Once tacked, a long seam is not welded in one pass from end to end. TWI gives two sequences. Back-step welding deposits short adjacent lengths in the direction opposite to the overall progress, so each segment ends against the one before. Skip welding deposits short, evenly spaced lengths in a set order, all in the same direction, with each length and gap about the natural run-out of one electrode.
A weld site, Material Welding, describes back-step welding as a way of working in reverse to the direction of travel, and adds that it lowers heat input and helps thin sheet that is prone to warping. It also says the method calls for more practice than a straight run. The site gives no segment length or other number, which fits TWI’s wording: the length comes from the electrode or the wire and the joint, not from a rule.
Both rest on one principle: weld toward the free end of the joint, never into a corner that cannot move, and to place the next segment where the panel is cool. TWI adds that on long welds the whole seam should not be completed in one direction.
- Tack at the ends and the middle first, then at shorter spacing along the joint.
- Weld the first segment away from the center, and the second where the panel has had time to cool.
- Keep the joint balanced about the neutral axis, with welds on both sides of a panel taken in alternation.
- Check the gap at the far end after each segment, before the seam closes.
TIG, MIG or Spot Welding for Thin Sheet
The process changes the amount of heat the panel receives. TWI advises depositing weld metal quickly with the fewest runs, using the largest electrode diameter or highest current that does not cause lack of fusion, and preferring MIG to manual metal arc welding. It adds that mechanized welding, with high deposition rate at high travel speed, gives the greatest distortion control, and that gas welding usually produces more angular distortion than arc processes.
Euroinox names TIG, plasma arc, MIG, SMAW and resistance welding as especially suited to stainless steel, and mentions stud welding, which fixes panels without weld clean-up or surface marking. It adds that the surface finish should be considered when choosing the process, because a directional finish needs restoring at welded junctions.
| Process | Where it fits | Published point |
|---|---|---|
| TIG | Stainless, aluminum and mild steel sheet where the seam is seen | Named among the processes suited to stainless (Euroinox) |
| MIG | Mild steel and stainless where speed matters | TWI prefers it to manual metal arc for distortion |
| Resistance spot welding | Overlapped sheet, enclosures, brackets | 8 to 15 kA for about one fifth of a second on steel (AHSS Insights) |
| Stud welding by capacitor discharge | Fixing panels and studs without surface marking | No weld clean-up (Euroinox) |
| Plasma arc | Stainless sheet | Named in the Euroinox list |
Spot welding limits heat by its short time. AHSS Insights gives the heat input as I²Rt, the square of the current times the total resistance times the time. It adds that a lobe curve defines the range of current and time that produces an acceptable nugget, that worn electrodes mushroom and lower the current density, and that for sheets of different thicknesses the parameters of the thinner sheet are used. Alternating current needs roughly 10 percent more energy than direct current for the same weld size, per the same source.
The practical effect is that a spot-welded flange moves less than a seam-welded one, but it needs overlapped sheet and access for two electrodes, so it is a design choice made before the parts are cut.
Welding Stainless and Aluminum Sheet
Stainless and aluminum bring their own conditions, and the producers print them. Cleveland-Cliffs, in its datasheets for 304 and 316, calls the austenitic stainless steels weldable by the common fusion and resistance techniques and warns that hot cracking is avoided by assuring formation of ferrite in the weld deposit. Fillers of AWS class 308, 308L or 347 are most often specified for 304, and 316L or 16-8-2 for 316.
| Alloy | Weldability statement | Filler or note | Source |
|---|---|---|---|
| 304 | Weldable by fusion and resistance techniques | AWS E/ER 308, 308L or 347; ferrite needed against hot cracking | Cleveland-Cliffs |
| 304L | Low carbon, immune to carbide precipitation from welding | Usable as-welded in severe service | Cleveland-Cliffs |
| 316 | Poorer weldability than 304, higher nickel | Slower arc speed; AWS E/ER 316L or 16-8-2 | Cleveland-Cliffs |
| 5052 aluminum | Sensitive to cracking with a base alloy filler; welded with 5356 or 5554, or 4043 | Filler guidance | ESAB, Lincoln Electric |
The 316 sheet datasheet gives the reason for the slower travel: its higher nickel content calls for a slower arc welding speed and more care against hot cracking. A thin 316 panel therefore takes more heat per length of seam than the same 304 panel, and it asks more of the sequence.
Cleveland-Cliffs also lists published procedure specifications by thickness band, for example gas tungsten arc welding of 300 series at 0.050 to 0.14 in (1.3 to 3.6 mm) and at 0.125 to 1.5 in (3.2 to 38 mm). A welding procedure is qualified for a thickness band, so a supplier that welds 1.5 mm stainless holds a different qualification from one that welds 6 mm.
Aluminum sheet in 5052 welds, but its filler is chosen with care. ESAB notes that alloys with 1 to 2.5 % magnesium, 5052 among them, are very sensitive to cracking when welded with a filler of their own composition, and that a 5 % magnesium filler such as 5356 raises the magnesium in the diluted weld and lowers that risk. Lincoln Electric gives 4043, 5554 or 5356 for 5052, with 5356 and 5554 the more common so one filler serves the shop, and says 4043 suits no other 5xxx alloy because 5052 alone has that low a magnesium content. Neither gives weld settings, so a procedure is written for the alloy and the thickness at hand, not carried across from steel.
Presetting, Clamping and Releasing the Part
Distortion that is certain can be used. When a seam always pulls a flange in by the same amount, the part is set the other way before welding, so the shrinkage brings it back to square. TWI says mechanized welding, with high deposition rate and high travel speed, gives the most consistent distortion and so makes presetting most effective. A hand-welded seam varies from one operator to another, and presetting to a figure that moves by a third is guesswork.
Clamping works the other way. A clamped panel cannot move, so the shrinkage stays in the metal as stress and comes out when the clamps are removed. TWI covers the same problem under back-to-back assembly: two identical parts held together are welded in balance, and stress relieving before separation is recommended, since otherwise the parts spring on release and wedges are needed to bring them back.
The sequence of the release matters as much as the sequence of the weld. A fixture that holds a box square during welding and is opened while the part is still warm lets the part relax out of square. A shop that holds a tolerance on squareness can release the clamps after cooling, or measure the part in the fixture and again out of it, and the two readings show how much stress the weld locked in.
Clamping hides distortion without removing it. The stress waits in the weld until the fixture opens.
TWI adds two more points for the procedure itself: keep fillet welds to the specified minimum size, since every extra millimeter of weld is shrinkage, and minimize the time between runs. A fillet drawn larger than the load needs is a fillet that bends the panel for nothing. When a welded assembly keeps fighting its own distortion, the alternative is a part with no seams: a small bracket or housing with several faces that have to stay square can often be made as machined aluminum from one block, trading the welding sequence for machining time.
Cut Edges and Cleaning Before the Torch
A weld starts at a cut edge. A laser cut in oxygen leaves an oxide layer at the edge, and the trade article in All About Industries says rework is needed on oxygen-cut parts that go to painting or galvanizing. The same oxide sits in the joint if the edge is welded as cut, and it enters the pool. Nitrogen-cut edges are bright and scale-free, so they go to the torch without cleaning.
SSAB asks that thermal cut and sheared edges be deburred and rounded with a grinder before the next operation. Dressing also removes burrs that stop panels from seating flat, and a panel that does not seat is a gap that closes during welding.
- Specify the cutting gas when the part is welded at the cut edge.
- Dress the edge where burrs would keep a panel from seating.
- Plan restoration of a brushed finish where a weld crosses it.
Checking a Welded Sheet Assembly
The last step of the sequence is to prove it. A welded assembly is judged against the drawing as a whole, so the order in which dimensions are measured should follow the order in which the part was built. Size comes first, then squareness, then flatness and hole position, because each later check depends on the earlier one holding.
Distortion shows in square, flatness and the position of mating holes. A drawing without a welding tolerance leaves the shop to choose, and many shops fall back on a general tolerance for welded structures. Kalmar’s old in-house K-standard on general welding tolerances, marked by its maker as not for new design, shows what such a document does: it gives permissible linear deviations by class from AA to D, such as plus or minus 2 mm in class B for dimensions between 30 and 315 mm, and states that it applies only when the standard and class are called out on the drawing.
The same document says deviations can be checked with simple instruments, a caliper, steel rule, measuring tape or square, if the measuring uncertainty is not more than one fifth of the tabulated tolerance. That ratio is a useful habit for any weld check.
- Measure the diagonals of a box, since equal diagonals show it is square.
- Check flatness on a surface plate with the assembly resting free, not clamped.
- Check hole positions after welding, since a hole that fit before welding can move.
- Retain the first welded piece as the reference for the run.
Orders that begin as a few welded prototypes and grow into hundreds pass through low-volume sheet metal work and into bridge production with the same tacking order, sequence and fixtures, so the first approved weldment sets how every later one is made.
Sources and Further Reading
- TWI, Distortion Control and Prevention by Fabrication Techniques (job knowledge 36). https://www.twi-global.com/technical-knowledge/job-knowledge/distortion-control-prevention-by-fabrication-techniques-036
- Material Welding, Back Step Welding. https://materialwelding.com/back-step-welding/
- Euroinox, Guide to Stainless Steel Finishes, Building Series, Volume 1 (weldability). https://www.imoa.info/download_files/stainless-steel/euroinox/Finishes.pdf?m=1454491282
- Cleveland-Cliffs, 304 / 304L Stainless Steel product data (weldability). https://www.clevelandcliffs.com/_assets/_55901e6ecec4b7127f2b520e9bb71227/clevelandcliffs/db/1190/10510/file/CLF_ProductData_304-304LSS_052021.pdf
- Cleveland-Cliffs, 316 / 316L Stainless Steel product data (weldability). https://www.clevelandcliffs.com/_assets/_44232ebbf32f67660c1d6a1104d40206/clevelandcliffs/db/1190/10513/file/CLF_ProductData_316-316LSS_052021.pdf
- AHSS Insights, Resistance Spot Welding. https://ahssinsights.org/processes/resistance-spot-welding/
- AHSS Insights, tag page on resistance spot welding heat balances (AWS C1.1 notes). https://ahssinsights.org/tag/rsw-heat-balances/
- Kalmar, K-standard 20024.0001, General tolerances, welding, edition 5 (fetched copy, URL not recorded).
- All About Industries, Cutting Gas in Laser Cutting. https://www.all-about-industries.com/how-oxygen-and-nitrogen-shape-the-cutting-edge-a-0998ffea9af2d4989ab8302169e219e5/
- Bending Hardox, SSAB
- 6 Key Factors to Choose the Right Aluminum Filler Metal, ESAB
- Welding Aluminum in the Trailer Industry, Lincoln Electric