A bending column in The Fabricator charts 3.2 mm (0.125 in) 5052 aluminum in the H32 temper at a minimum inside radius of zero to one thickness, while the same alloy in H38 carries about a quarter more tensile strength and less of the stretch a tight bend needs. Nothing changed but the temper. For steel the spread is wider still: Salzgitter rates its S355MC at a quarter of the thickness up to 3 mm and its S700MC at one and a half, a sixfold difference within one product standard.
A minimum bend radius is therefore never a property of “sheet metal”. It belongs to one grade, one temper, one thickness band, one bend angle and one direction of bending relative to rolling, and the radius that appears on a drawing is usually not the minimum at all but the one the press brake die forms by itself. The sections below take the makers’ figures in that order: what the minimum is, what a die actually produces, and what changes both.
Minimum Inside Bend Radius Values for Steel Sheet
Steel makers print the minimum as a multiple of thickness, t, and the multiple rises with strength and with thickness. The two hot-rolled cold-forming ranges below are the clearest published sets; mild cold-rolled steels such as DC01 come with formability figures but, in the makers’ datasheets cited here, no printed radius.
| Grade, maker and condition | Multiple at 2 mm | Radius at 2 mm (0.079 in) | Multiple at 5 mm | Radius at 5 mm (0.197 in) |
|---|---|---|---|---|
| S355MC, Salzgitter, bends up to 90° | 0.25 t | 0.5 mm (0.020 in) | 0.5 t | 2.5 mm (0.098 in) |
| SSAB Domex 355MC, 90° bend | 0.2 t | 0.4 mm (0.016 in) | 0.3 t | 1.5 mm (0.059 in) |
| S420MC, Salzgitter, bends up to 90° | 0.5 t | 1.0 mm (0.039 in) | 1.0 t | 5.0 mm (0.197 in) |
| SSAB Domex 420MC, 90° bend | 0.4 t | 0.8 mm (0.031 in) | 0.5 t | 2.5 mm (0.098 in) |
| S500MC, Salzgitter, bends up to 90° | 1.0 t | 2.0 mm (0.079 in) | 1.5 t | 7.5 mm (0.295 in) |
| S700MC, Salzgitter, bends up to 90° | 1.5 t | 3.0 mm (0.118 in) | 2.0 t | 10.0 mm (0.394 in) |
Salzgitter’s thickness bands are up to 3 mm, over 3 to 6 mm, and over 6 mm; SSAB’s are 1.80 to 3.00, 3.01 to 6.00 and 6.01 mm and up. Its figures follow EN 10149-2 and apply in both the longitudinal and transverse directions; SSAB states its bending properties for both directions too. Radii in millimeters are the multiple times the thickness.
Two patterns repeat in every maker’s table. The multiple steps up with each thickness band, so a 5 mm part is not a 2 mm part scaled. And the higher the yield strength, the larger the multiple, so a part redesigned in a stronger grade to save weight usually needs its radii redrawn.
A minimum radius is a statement about one grade at one thickness. Copied from one part to another, it is a guess.
Mandrel Diameter and Radius
EN 10149-2 states its bending requirement differently again. ArcelorMittal prints it as the minimum mandrel diameter for a 180 degree bend: 0.5 t for S355MC and S420MC, 1 t for S460MC and S500MC and 1.5 t for S550MC and S600MC. A diameter of 0.5 t is a radius of 0.25 t, and a 180 degree bend is a harsher test than a 90 degree one. Figures from a 180 degree mandrel test and from a 90 degree recommendation are not interchangeable on a drawing.
Minimum Radius and the Radius a Die Forms
The minimum is what the material survives. It is rarely what the part should be drawn with. An article in The Fabricator on minimum and recommended radii draws the line clearly: the minimum inside radius is what is physically possible with enough press tonnage, and the recommended radius is what gives the best results and the most stable bend angles. For 0.5 in (12.7 mm) plate it describes a recommended die opening of 10 times the thickness, giving close to a one-to-one radius, and warns against forcing the plate into a die only five times as wide.
In air bending the radius is set by the die, not by the punch. Wila puts it as a natural product radius that depends mainly on the V-opening, and gives a rule of thumb for steel of about 450 N/mm² (65 ksi) tensile strength: a V-opening of 6 to 8 times the thickness for sheet up to about 3 mm, which forms a 90 degree bend with an inside radius approximately equal to the thickness. Bystronic gives the same idea as a number: mild steel air-bends to an inside radius of about 16 % of the V-opening.
| Thickness | V-opening | Inside radius formed | Radius as a multiple of t |
|---|---|---|---|
| 1.0 mm (0.039 in) | 8 mm (0.31 in) | about 1.3 mm (0.05 in) | 1.3 t |
| 1.5 mm (0.059 in) | 12 mm (0.47 in) | about 2.0 mm (0.08 in) | 1.3 t |
| 2.0 mm (0.079 in) | 16 mm (0.63 in) | about 2.6 mm (0.10 in) | 1.3 t |
| 3.0 mm (0.118 in) | 25 mm (0.98 in) | about 4.0 mm (0.16 in) | 1.3 t |
| 5.0 mm (0.197 in) | 40 mm (1.57 in) | about 6.5 mm (0.26 in) | 1.3 t |
| 8.0 mm (0.315 in) | 63 mm (2.48 in) | about 10.0 mm (0.39 in) | 1.25 t |
| 10.0 mm (0.394 in) | 80 mm (3.15 in) | about 13.0 mm (0.51 in) | 1.3 t |
The chart applies to mild steel of about 450 N/mm² (65 ksi) tensile strength in 90 degree air bending, with the V-opening at about eight times the thickness. Durmapress calls the values widely accepted reference values that vary with material batch, tooling condition and machine calibration, and asks for a test bend before production.
Set beside Table 1, Table 2 shows the gap a drawing has to cross. At 2 mm, S355MC is allowed a radius of 0.5 mm, but the die that bends it most consistently forms about 2.6 mm. A drawing that calls the minimum asks for a narrow die, more force and less stable angles; a drawing that calls the die-formed radius gets the machine’s best work.
The Punch Tip Does Not Set the Radius
In air bending the punch tip follows the sheet rather than shaping it. Durmapress gives the example of mild steel bent in a 32 mm (1.26 in) V-opening: whether the punch tip radius is 0.8 mm or 2 mm, the inside radius comes out at about 5.1 mm (0.20 in), 16 % of the opening. The tip still matters at the other extreme. Bystronic warns that thick or high-tensile sheet tends to crease, crack or split under a narrow punch tip combined with a narrow die, and advises consulting the material supplier on the punch tip radius for challenging applications above 0.5 in (12.7 mm).
Its own starting set is modest: an acute offset knife punch with a 0.04 in (1.0 mm) radius for material 0.187 in (4.75 mm) and thinner, and a straight punch with about a 0.120 in (3.0 mm) radius for 0.187 to 0.5 in. A punch radius smaller than the material’s minimum radius is where the crease begins.
Getting a Smaller Radius From the Die
Narrower dies give tighter radii, within limits. Bystronic’s example takes 0.125 in (3.2 mm) mild steel: a 1 in die forms about a 0.16 in (4.1 mm) radius, and a 0.75 in die about 0.12 in (3.0 mm), close to one thickness. Its limit is plain.
A V-opening below five times the thickness compromises angular accuracy, can damage the machine and tooling, and is unsafe. Wila draws the line at six times the thickness for steel, below which the radius cannot form properly, the force rises sharply and the die flanks wear or may split.
- Radius larger than the die forms: a wider die, which also lowers the force and the marking on the sheet, and lengthens the minimum flange.
- Radius about equal to the die’s natural radius: the standard die, the most repeatable angle.
- Radius below the natural radius but above the minimum: a narrower die down to five or six thicknesses, more force, less consistent angle.
- Radius at or below the material minimum: a crack risk at the outside of the bend, whatever the die.
Rolling Direction and Bend Orientation
Sheet carries the direction of the mill in its grain. A Fabricator article on heavy bending explains that rolling stretches the metallurgical structure and inclusions along the rolling direction, so a bend line running with the grain, a longitudinal bend, opens the grains on the outside and cracks there first. Bending across the grain needs more force but accepts a much tighter radius.
The same publication gives an example from plate: grades 350 and 400 between 0.5 and 0.8 in (12.7 and 20.3 mm) thick may have a minimum radius of 2.5 t when bent transversely and 3.75 t longitudinally. Wila lists rolling direction alongside tensile strength and ductility among the material properties that set the minimum radius.
Thin cold-forming grades narrow that gap on purpose. Salzgitter describes its MC grades as having bending properties in both directions, and SSAB states its Domex radii for both. For a grade that does not print both, the nest is where the direction is decided. A part laid out with its tightest bend across the rolling direction gets the more forgiving condition, and a drawing that marks the rolling direction on that part tells the programmer.
Estimating a Minimum When No Table Exists
Where a datasheet gives no radius, The Fabricator’s columnist describes a rough rule based on the tensile reduction percentage the material supplier specifies: divide 50 by that percentage, subtract 1, and multiply by the thickness. The article is explicit that this is a rough guide, that actual minimum values vary by grade, and that the material supplier’s data is the place to look first. Any value it gives is a minimum, so the die-formed radius of Table 2 still sits above it on the drawing.
Cut Edges Before the Bend
Thermal cutting changes the edge the bend starts from. The heavy-bending article notes that flame and laser cutting harden the edge and produce stress concentrations, and that dressing sheared edges and removing surface gouging can reduce microfractures in critical areas. A crack at the outside of a bend often begins at the corner where the cut edge meets the bend line, which is why a bend relief or a slightly larger radius at the edge helps a tight bend survive.
Aluminum Bend Radius by Temper and Thickness
Aluminum shows the temper effect more sharply than steel, because its tempers are made by cold work and each step of hardening takes ductility away. The Fabricator’s column on predicting an air-formed bend radius works with tensile strengths of 33,000 psi (228 MPa) for 5052-H32, 38,000 psi (262 MPa) for H34, 40,000 psi (276 MPa) for H36 and 42,000 psi (290 MPa) for H38, values it takes from a materials database. For the minimum, the same column prints a chart that gives 0 to 1 times the thickness for 0.125 in (3.2 mm) 5052-H32, beside a reader’s note that the supplier suggested at least 1.5 times for the same sheet, and its advice is to check the recommended minimum with the material supplier.
| Temper | Tensile strength, MPa (psi) | Inside radius at 3.2 mm (0.125 in) |
|---|---|---|
| O, annealed | elongation 20 %, 148 MPa (21.5 ksi) between yield and tensile | not quoted |
| H32 | 228 (33,000) | 0 to 1 t, 0 to 3.2 mm (0 to 0.125 in), in the column’s chart; 1.5 t, 4.8 mm (0.19 in), the supplier’s suggestion |
| H34 | 262 (38,000) | not quoted |
| H36 | 276 (40,000) | not quoted |
| H38 | 290 (42,000) | not quoted |
The two H32 figures differ by half a thickness, which on a 3.2 mm part is 1.6 mm (0.063 in) of radius. Neither is a guaranteed value: the minimum that governs a part is the one in the product specification or the supplier’s table for that temper, thickness and bend direction, confirmed by a trial bend.
Why Temper Moves the Radius
The column defines the minimum radius as the point at which cracks start to appear on the outside surface of the bend, where the grains begin to separate, and it ties the limit to ductility. From a tensile test it takes the reduction of area, r, the percentage by which the specimen’s cross section shrinks at fracture, and gives the minimum inside radius as the thickness times (50 / r − 1). A reduction of area of 25 % gives one thickness, and 50 % gives zero.
Its column on formable aluminum reads formability the same way, as elongation and the gap between yield strength and tensile strength. In the annealed temper it gives 5052 an elongation of 20 % and a gap of 21.5 ksi, and it notes that aluminum work-hardens as it is bent. Each H temper starts that hardening before the part reaches the brake, so the harder the temper, the less stretch is left for the outside of the bend. Elongation and reduction of area on a mill certificate are the quickest figures for judging whether a tight radius will hold.
Heat-Treatable Alloys
Hydro’s guide to aluminum alloys for bending ranks 3003 and 5052 as the easiest, with 5052 in the O temper beating 3003 in formability. For heat-treatable 6061 and 6082, it recommends bending in the T4 temper and heat treating to T6 afterward where the process allows, because bending capacity falls significantly in T6. It adds a caution about T4: its yield strength rises slowly at room temperature through natural aging, which can make springback inconsistent.
The Fabricator’s heavy-bending article gives plate figures from a material supplier that show the same trend: 6061 in the O condition at 1 t for 0.25 in (6.4 mm) plate, 1.5 t at 0.375 in (9.5 mm) and 2 t at 0.5 in (12.7 mm); in T4, 3 t, 3.5 t and 4 t at the same thicknesses; and 7050 at 0.5 in up to 9.5 t. It also says that aluminum harder than 5054 needs annealing along the bend line before heavy bending, or it will crack.
In aluminum, temper moves the minimum radius further than thickness does. The temper on the drawing is part of the radius.
Stainless Steel and High-Strength Steel at the Brake
Stainless steel brings its own pair of facts. Cleveland-Cliffs describes annealed 304 and 304L as very ductile and easily bent, but notes that the material work hardens rapidly, so in-process annealing may be needed in severe forming. The die sets its radius as for steel, but with a wider opening: the Durmapress chart gives 10 to 12 times the thickness for 304 of about 600 N/mm² (87 ksi) tensile strength, and an inside radius of 20 to 22 % of the opening. That works out at about 2.0 to 2.6 t for a standard air bend, roughly double mild steel’s 1.3 t.
High-strength steel moves further. Durmapress gives 12 to 20 times the thickness for grades above 800 N/mm² (116 ksi), and Wila says such materials could easily need more than 12 to 15 times. Since the formed radius is a fraction of the opening, a high-strength part bent in a wide die gets a large radius whether the drawing asks for one or not.
- Mild steel, about 450 N/mm²: V of 8 t, radius about 16 to 17 % of V, about 1.3 t.
- Stainless 304, about 600 N/mm²: V of 10 to 12 t, radius 20 to 22 % of V, about 2.0 to 2.6 t.
- Aluminum 5052, soft: V of 5 to 6 t, radius 13 to 15 % of V, about 0.7 to 0.9 t.
- High-strength steel above 800 N/mm²: V of 12 to 20 t, radius not fixed in the chart.
The multiples in the right-hand figures are the chart’s two columns multiplied together, for a buyer’s first estimate; the tooling maker’s specification governs.
Heavy Plate and Heat
For very thick plate, the heavy-bending article suggests preheating to 200 to 300 °F (93 to 149 °C) before tight bends, particularly at 0.75 in (19 mm) and above, with uniform heating. That is far outside thin sheet work, but it marks the point where cold bending to a tight radius stops being a press setting and becomes a process change.
Checking the Bend Radius on the Drawing and the First Part
A radius on a drawing is checked twice: once against the material’s minimum, and once against the die the shop will use. The first check is a datasheet lookup with the right grade, temper, thickness band and direction. After that comes a question for the bending shop, because the flat pattern depends on it. Autodesk’s Inventor documentation notes that a bend table built for a particular machine needs measured sample pieces for each cell to be accurate, and that a part with only 90 degree bends of one radius gains nothing from a bend table over a K-factor.
For the first part itself, the radius is measured with a radius gauge or a profile at the inside of the bend. Bystronic notes that bends in sheet metal have slightly elliptical corner radii, so a measurement only has to come close, and that a nominal 0.250 in die in metric tooling is actually 6 mm (0.236 in), which shifts the radius a little between tool systems. Wila adds that makers do not all measure the V-opening the same way; it measures between the virtual intersections of the bearing faces and the groove.
After measurement, the outside of every tight bend is inspected for cracking, orange peel or splitting at the edges. A first part bent along and across the rolling direction, where the nest allows both, shows which orientation the material tolerates before the batch is cut.
Brackets and enclosures whose radii are still being settled suit low-volume sheet metal, where the die-formed radius of the first piece becomes the radius on the drawing, and the flat pattern that goes with it is what a later bridge production batch is cut to.
Minimum radii for thin stainless and for mild cold-rolled steel are not printed in any of the makers’ datasheets cited here, so for those materials the die-formed radius and a test bend remain the working evidence.
Sources and Further Reading
- High-Strength Steels for Cold-Forming, Thermomechanically Rolled, Salzgitter Flachstahl
- SSAB Domex 355MC, meets S355MC, SSAB
- SSAB Domex 420MC, meets S420MC, SSAB
- A20, Amstrong High Strength Steels, ArcelorMittal
- Predicting an Air-Formed Sheet Metal Inside Bend Radius, The Fabricator
- Formable Aluminum: Press Brake Bending 6061 With the 20% Rule, The Fabricator
- Here Are the Best Aluminium Alloys for Bending, Hydro
- 304/304L Stainless Steel, Product Data Bulletin, Cleveland-Cliffs
- Press Brake V Die Opening Chart, Rule of 8, Radius and Tonnage, Durmapress
- The Rules of Press Brake Tool Selection, Bystronic
- V-Opening, Wila
- Minimum Inside Sheet Metal Bend Radius and What Is Recommended, The Fabricator
- Bending Basics, The Fundamentals of Heavy Bending, The Fabricator
- About Bend Tables for Sheet Metal Materials, Inventor 2024 Help, Autodesk