AluminumStainless SteelCoil

Press Brake Bending of Sheet Metal From Die Opening to Final Angle

A press brake bend is decided by the die opening, which sets radius, flange length, springback and the flat pattern, so the first piece carries every assumption of the lot.

A bent stainless steel sheet bracket resting in a plain steel press brake V-die with the punch tip just above it.

Bystronic’s tooling guide opens with a plain example: a plate 0.125 in (3.2 mm) thick wants a die opening 1 in (25.4 mm) wide, and the flange it forms then has to be at least 0.77 in (19.6 mm) long. A shorter flange has nothing to rest on, so it drops into the groove instead of bending against it. One thickness sets a die, the die sets a radius and a minimum flange, and the radius sets the length of the flat pattern the laser cut an hour earlier.

That chain explains why a bent bracket can come off the brake at the wrong size with every cut dimension correct. The sections below follow a bend from the choice of die opening to the last angle check, with the numbers the tooling makers and the sheet metal references print.

How a Press Brake Forms a Bend in Air

Most sheet metal is bent by air forming. The punch pushes the sheet into a V-shaped die, and the sheet touches only three points: the two shoulders of the die and the tip of the punch. Ram travel, not the shape of the groove, sets the angle, so one die serves many angles.

Wila describes air bending in exactly these terms: a range of angles from a limited tool set, with springback easier to compensate for than in other methods. It also notes that the inside radius of the finished part is set mainly by the width of the die opening, and that the punch tip radius should sit as close to the material’s natural radius as possible without exceeding it.

Two harder methods exist. Bottoming presses the sheet into the groove until it matches the angle of the die, and coining squeezes it past that point. Both need more force than air forming, since the press then has to crush the material and not just fold it. Durma’s K-factor table lists separate values for the three methods, and that is a hint of how different the stress states are.

The sheet touches the die at three points. Ram depth sets the angle, die width sets the radius.

Choosing a V Die Opening for the Sheet Thickness

Bystronic states the rule of eight: the V opening should be eight times the thickness, then rounded to the nearest die the shop owns. For 0.125 in material that is 1 in. A shop that bends from 0.030 in (0.76 mm) to 0.250 in (6.4 mm) needs at least four dies, at 0.25, 0.5, 1.0 and 2.0 in, each double the last.

The rule is a starting point for mild steel, and other alloys move it. Durma’s chart gives a different multiple for each material.

Table 1. Starting V opening and formed inside radius for 90 degree air bending, from Durma’s V-die guide
Material V opening as a multiple of thickness Inside radius as a share of the V opening
Mild steel about 8 about 16 percent
Stainless steel 10 to 12 20 to 22 percent
Aluminum 5052 5 to 6 13 to 15 percent
Aluminum 6061-T6 10 to 12 13 to 15 percent
High-strength steel above 800 N/mm² (116 ksi) 12 to 20 not specified

Wila gives 6 to 8 times thickness for steel up to about 3 mm (0.12 in) and warns that high-strength steels often want more than 12 to 15 times. The two limits on the narrow side are firm. Bystronic says a die narrower than five times the thickness harms angular accuracy and risks damage to the machine and tooling. Wila says a V under six times thickness raises force sharply and wears the die flanks.

Die sizes also differ between inch and metric tooling. Bystronic notes that a nominal 0.250 in opening is a 6 mm (0.236 in) die in the metric standard, so a drawing built for one system and bent on the other can change the radius by a few hundredths of a millimeter, enough to move a tight flat pattern.

A wide die costs something too. Wila points out that a larger V gives a larger radius and less friction marking, but any change of V changes the flat pattern, which is costly to correct once parts are cut.

Inside Radius and Minimum Flange Length From the Die

The radius a bend takes is a result of the die, not a choice made on the drawing. Bystronic gives 16 percent of the opening for air-bent mild steel, so a 1 in die yields about a 0.16 in radius. For 90 degrees, Wila notes the natural inside radius is roughly equal to the sheet thickness, which is where the rule of eight comes from: an opening of eight thicknesses at 16 percent gives 1.3 thicknesses.

Table 2. Mild steel air bending at 90 degrees, die opening and the radius and flange it implies
Thickness V opening Inside radius Minimum flange at 0.77 of V
1 mm (0.039 in) 8 mm (0.31 in) about 1.3 mm (0.05 in) 6.2 mm (0.24 in)
2 mm (0.079 in) 16 mm (0.63 in) about 2.6 mm (0.10 in) 12.3 mm (0.48 in)
3 mm (0.118 in) 25 mm (0.98 in) about 4.0 mm (0.16 in) 19.3 mm (0.76 in)
5 mm (0.197 in) 40 mm (1.57 in) about 6.5 mm (0.26 in) 30.8 mm (1.21 in)
8 mm (0.315 in) 63 mm (2.48 in) about 10.0 mm (0.39 in) 48.5 mm (1.91 in)

Thicknesses, openings and radii come from Durma’s mild steel chart for steel of about 450 N/mm² (65 ksi) tensile strength; the flange column applies the 0.77 factor that both Bystronic and Durma print, and the arithmetic is the writer’s own. Durma adds that the tooling maker’s own specification governs.

Three consequences follow for a buyer who draws a part.

  • A flange shorter than about three quarters of the die opening cannot be formed in a standard die. A part with a short return lip needs a narrow die, a different radius or a different method.
  • A hem, bent in two stages, needs at least 115 percent of the opening, because of the 30 degree prebend, per Bystronic.
  • A hole too close to a bend stretches into an oval. Bystronic’s rule of thumb places holes at least six thicknesses from the bend line, and the flange itself at least six thicknesses long.

Drawing a 1 mm inside radius on a 3 mm steel part asks for a die the shop cannot use without cracking the sheet or changing the thickness.
A short example shows how the pieces connect. Take a 2 mm (0.079 in) stainless bracket with a 90 degree flange is drawn with a 2 mm inside radius. Durma’s multiples for stainless put the die at 20 to 24 mm and the formed radius at 20 to 22 percent of that opening, so the die the shop reaches for gives 4.0 to 5.3 mm (0.16 to 0.21 in), about twice the drawn radius. The drawing and the die disagree before any metal moves, and the shop either asks, or bends to the radius its tooling gives.

The reverse case is easier to miss. A radius drawn larger than the die gives is formed with a tighter tool and a deeper stroke, and the part leaves with the radius the die made. Neither bend shows on the cut file, so the radius belongs on the drawing as a limit the buyer can accept, for example a range, and not a single number.

Springback and the Overbend That Cancels It

When the punch lifts, the sheet relaxes. SSAB describes springback as the material trying to return to its original shape after it is bent, and its Hardox bending brochure adds that all springback is fully elastic, controlled by the level and distribution of plastic strain in the bend. The recovered angle is the springback, and the operator corrects for it by bending past the target, so the die’s opening angle has to leave room for that overbend without bottoming out.

Table 3. Springback calculated by SSAB for a 90 degree bend along the rolling direction, by grade and thickness, with the press force per meter of bend
Grade 5 mm (0.20 in.) 10 mm (0.39 in.) 15 mm (0.59 in.)
SSAB Domex 355MC 3.9°, 310 kN/m (1,770 lbf/in.) 3.9°, 630 kN/m (3,600 lbf/in.) 3.9°, 950 kN/m (5,420 lbf/in.)
Strenx 700MC 6.7°, 570 kN/m (3,250 lbf/in.) 6.9°, 1,170 kN/m (6,680 lbf/in.) not given
Strenx 1100E 14.2°, 820 kN/m (4,680 lbf/in.) 16.3°, 1,340 kN/m (7,650 lbf/in.) 16.2°, 2,010 kN/m (11,480 lbf/in.)
Hardox 450 14.8°, 860 kN/m (4,910 lbf/in.) 16.6°, 1,380 kN/m (7,880 lbf/in.) 16.5°, 2,070 kN/m (11,820 lbf/in.)

The table runs from a 355 MPa structural grade to a wear steel, and the springback grows about fourfold across it. SSAB states that springback increases with the strength of the steel and with the ratio of die width to thickness, and that yield strength has the biggest influence. Its brochure lists the other parameters: a larger punch radius and a wider die both raise springback, and so does the strain hardening of the material. For sheet under 10 mm (0.394 in.) it gives a rough estimate, the tensile strength in MPa divided by 100, as degrees of springback, and it warns that the figure depends to a large extent on each tool setup, so trials come first.

The practical reading is that a part with a generous radius is harder to hold to an angle than one with a tight radius. A bracket in 304 with a 90 degree bend and a 2 to 3 degree recovery needs the brake to close to about 87 degrees to land at 90, and the control learns that offset from the first piece.

The angle also depends on the lot. Two coils of the same grade differ in yield, and a part made from the second coil can open a half degree from the first. For that reason a tolerance on bend angle is read at the first piece of each lot, and the setup is adjusted before the run begins.

Bending Force and What It Limits

Force sets which brake can make a part, and it reacts strongly to the die. Durma prints an estimate for 90 degree air bending: force in kN equals bend length times thickness squared times tensile strength times 1.42, divided by the V opening times 1,000, with lengths in mm and strength in N/mm². Take 1,000 mm of 2 mm mild steel at 450 N/mm² over a 16 mm die. The result is about 160 kN, close to 16 metric tons-force on a 1 m (39 in) bend.

Two statements from Durma matter more than the number. Doubling the V opening cuts the force by roughly half, and the material changes it by a factor: stainless needs 1.4 to 1.5 times mild steel, aluminum 5052 only 0.5 to 0.6 times, and high-strength steel 2.0 to 3.0 times. Durma also warns that the machine and the tooling each carry a load rating, and that both have to be checked.

Bystronic adds a case that surprises buyers. Offsets and forming tools that reach into a narrow web can need about three times the standard air bending force, and its tool tolerance of 0.0004 in (0.01 mm) shows how tightly the tooling itself is ground. A long bend in thick stainless is therefore the first job to look at when a brake has to be chosen.

Bend Allowance and K-Factor for the Flat Pattern

The flat pattern has to be longer than the sum of the two flanges, since material at the bend stretches. Durma gives the bend allowance as BA = (π ÷ 180) × A × (R + K × T), with A the bend angle in degrees, R the inside radius, T the thickness and K the K-factor, the position of the neutral line in the thickness.

K depends on material, thickness, radius and method, and no single value covers a shop. Durma’s reference table starts air bending at 0.33 for soft material when the radius is under one thickness, 0.40 to 0.45 between one and three thicknesses, and 0.50 above three thicknesses. Bottoming sits higher in the same table and coining sits between the two. Durma’s worked example uses 0.43 for medium steel at a radius of 1.2 times the thickness.

Take a 90 degree bend in 2 mm mild steel, inside radius 2.6 mm from Table 2, with K at 0.43. The allowance is 1.5708 × (2.6 + 0.86), which is 5.4 mm (0.21 in). Flanges of 30 mm and 40 mm measured to the tangent points give a flat length of 75.4 mm (2.97 in). Change K to 0.40 and the flat shrinks by 0.1 mm, which is why the shop that cuts the blank also bends the first piece.

Durma states the reference values are starting points to validate by test bend on the actual material and tooling.

The shop records the K-factor with the material lot, die and punch. A repeat order holds the same value, or the flat pattern changes silently. Changing the die width calls for a fresh measurement, since V and radius move together.

Grain Direction, Cut Edges and Cracking

Sheet rolled in a mill has a grain, and a bend across it behaves differently from a bend along it. SSAB explains why: in many metals the grains are elongated in the rolling direction, so the material usually bends better transversely, across it. Its recommendations therefore give a separate minimum inner radius for each direction, and its Hardox brochure advises orienting the rolling direction transverse to the bend line where possible, since the plate can often be bent tighter that way. A smaller radius than recommended raises the risk of cracking. Wila adds that the smallest formable radius depends on tensile strength, ductility and rolling direction.

Cut edges join the problem. SSAB’s preparation list asks that thermal cut and sheared edges be deburred and rounded with a grinder before bending. A flame or oxygen cut edge on thick plate is also oxidized, as the gas choice in laser cutting explains, and an oxide edge at the outside of a tight bend starts cracks sooner than a clean one.

The visible symptoms of a poor bend are few.

  • Fine cracks or an orange-peel texture on the outer radius point to too tight a radius or the wrong grain direction.
  • A flange that is not straight or an angle that changes along the bend points to uneven die wear or a die set too narrow.
  • Witness marks along the bend line come from a narrow die or sharp shoulders, and lessen as V widens.

What the First Bend Has to Prove on a New Part

A first piece is cheap to check, and it carries every assumption of the setup. Check it before the lot runs.

  • Measure the angle on both ends of every bend, with a protractor or an angle gauge.
  • Measure the flat dimensions to the outside of the flanges, against the drawing.
  • Look at the outer radius at 10 times magnification for cracks.
  • Record die width, punch radius, bend angle at the control and the K-factor.

A second piece from the opposite end of the lot, bent after the setup has warmed and the operator has changed, shows whether the first one was luck. When the two agree within the angle tolerance on the drawing, the setup is stable enough to run.

Short runs that start as a handful of bent parts and grow to a few hundred pass through low-volume sheet metal work and into bridge production on the same die, K-factor and angle record that approved the first piece.

Sources and Further Reading

Request a Sheet Metal Quote

Send the 2D drawing and the 3D file, with the quantity and the stage of the project. An engineer replies within 1 working day.

The quote form, the mutual NDA and the private folder for your files are on Protolis Atelier, with Sheet Metal chosen.

Request a Quote