An M6 steel nut pressed into cold-rolled steel takes 27 to 36 kN (6,070 to 8,090 lbf) of press force to seat. Once it is in, PennEngineering’s bulletin for its S and CLS nuts credits it with a pushout resistance of 1,760 N (396 lbf), roughly one twentieth of the squeeze that put it there. That ratio is the whole character of the joint. The press does not drive the nut through the sheet; it makes the sheet flow, and the small amount of metal that flows into the nut’s undercut is all that holds it against a push from behind.
Every step of the insertion exists to protect that small volume of displaced metal. The hole has to leave it in place, the sheet has to be soft enough to move, the tooling has to squeeze it evenly, and the finish has to be on the panel before the nut goes in. This sequence follows the order of work on the shop floor, with the figures the fastener maker prints for each step.
How a Self-Clinching Nut Locks Into Thin Sheet
Installation takes three moves. First a hole of the specified size is punched or drilled, the nut’s shank is placed in it, and a press squeezes nut and sheet between parallel surfaces until the head meets the sheet. PEM’s installation instructions for its nuts, its miniature fasteners and its general do’s and don’ts all use the same three steps, and none of them includes deburring the hole.
What happens inside the squeeze explains the rest. The sheet around the head cold flows into an annular undercut in the shank, and a serrated clinching ring or knurl embeds in the sheet so the nut cannot turn when a screw is tightened into it. From then on the fastener is part of the panel. Its reverse side stays flush, with no swaged rim, because the clinch forms on the fastener side of the sheet.
| Step | What the maker specifies | What goes wrong | How it is seen |
|---|---|---|---|
| Check the sheet | Ductile, softer than the fastener, annealed condition, at least the minimum thickness for the shank code | Sheet too hard or too thin | Nut spins or pushes out at low load on the first test |
| Make the hole | Specified diameter, held to +0.08 mm (+0.003 in), no deburring, no chamfer | Oversize, chamfered or deburred hole | Clinching ring not fully embedded, low pushout |
| Place the nut | Shank inside the hole before force is applied, preferably from the punch side | Shank resting on the hole edge | Cocked head, sheared edge, distorted thread |
| Squeeze | Parallel punch and anvil, steady force until the head contacts the sheet | Hammer blow, uneven or excessive force | Gap under the head, crushed head, buckled sheet |
| Confirm | Seating judged by eye, force set by test before production | Force copied from the table without a trial | Lot-to-lot variation in pushout and torque-out |
The table reads as a chain. A wrong hole cannot be corrected by more force, and more force on a correct hole buckles the sheet. Most rejected installations trace back to a decision made before the press closed.
The nut is held by the sheet metal it displaces. Every step before the squeeze either keeps that metal available or removes it.
The Nut Families a Buyer Meets
PEM’s selector guide sorts its nuts by the sheet they go into. Its S and SS types serve steel or aluminum sheet, the CLS and CLSS types the same sheets where a stainless fastener is wanted, CLA nuts aluminum, and SP nuts stainless steel sheet. SMPS and SMPP nuts serve thin sheet and positions close to an edge, and SH nuts are made from hardened alloy steel for high-strength sheet. Locking versions add a prevailing-torque or free-running locking feature to the same clinching principle. A clinch nut gives thin sheet the thread that a thicker part would carry in its own wall: where a panel would need many threads or a thread deeper than the sheet allows, the part is often drawn as machined aluminum with tapped holes instead.
Sheet Hardness and Thickness Before Any Hole Is Cut
Hardness of the sheet decides which nut can be used at all. The clinch works only when the sheet is the softer partner, and an ASSEMBLY magazine article reprinted by PEM puts the rule of thumb at 20 points on the Rockwell B scale between panel and fastener. PEM’s bulletin then sets a ceiling for each nut type, and the ceiling falls as the fastener gets softer.
| Nut type | Fastener material | Sheet it is meant for | Maximum sheet hardness |
|---|---|---|---|
| S, SS | Carbon steel | Steel or aluminum | HRB 80, HB 150 |
| CLS, CLSS | 300 series stainless steel | Steel or aluminum | HRB 70, HB 125 |
| CLA | Aluminum | Steel or aluminum | HRB 50, HB 82 |
| SP | Hardened stainless steel | Stainless steel | HRB 90, HB 192 |
| SMPP | Stainless steel | Stainless steel | HRB 90, HB 192 |
| SH | Hardened alloy steel | High-strength steel | Tested in S700MC at HRC 23 |
The bulletin’s dos list adds that the panel should be in the annealed condition. A sheet that has been cold worked locally, by a bend or a coined feature, is harder there than its certificate says, and the bulletin’s note says fasteners should not sit adjacent to bends or other highly cold-worked areas.
Stainless Sheet and Stainless Nuts
Stainless sheet is where the rules tighten. PEM’s general guidance says a 300 series stainless nut is not to be installed into stainless sheet, and its bulletin limits stainless sheet to the SP and SMPP types, which are hardened for it. A Machine Design article by a PennEngineering manager adds the mechanism: installation in stainless can work-harden the material round the hole, which stops the displaced metal from flowing as intended. That is why the same bulletin asks for a sharp hole punch and, for SP nuts, a punch no more than 0.025 mm (0.001 in) above the minimum recommended hole.
Minimum Thickness and the Shank Code
Each nut comes in shank lengths coded 00 to 3, and each code sets a minimum sheet thickness. For an M6 nut the bulletin lists 0.92 mm for code 00, 1.2 mm for code 0, 1.4 mm for code 1 and 2.29 mm for code 2 (0.036, 0.047, 0.055 and 0.090 in). The recommended shank is always shorter than the minimum sheet thickness, so the force of installation does not reach the threads. For maximum performance, PEM recommends the longest shank the sheet thickness allows.
Thin sheet has its own floor. The Machine Design article puts the usual minimum at 0.76 mm (0.030 in), with some fasteners working in sheet as thin as 0.51 mm (0.020 in), and notes there is usually no maximum. Specialized micro fasteners go further: PEM’s MSOFS flaring standoffs install in panels 0.2 to 0.3 mm (0.008 to 0.012 in) thick, with their own flaring tool.
Hardness picks the nut type and thickness picks the shank code. Both are read off the material certificate before the nest is cut.
Mounting Hole Size, Edge Distance and Bend Clearance
The hole is the one dimension the nut cannot forgive. PEM prints a recommended hole for each thread with a tolerance of +0.08 mm and nothing below (+0.003 in, −0), and the ASSEMBLY article quotes the same band. Undersize, the shank will not enter or the sheet shears as it is forced in. Oversize, there is less metal to flow into the undercut.
| Thread | Hole in sheet, +0.08 mm | Minimum sheet, shank code 1 | Head diameter E | Minimum hole centerline to edge |
|---|---|---|---|---|
| M3 × 0.5 | 4.22 mm (0.166 in) | 1.0 mm (0.039 in) | 6.35 mm (0.250 in) | 4.8 mm (0.19 in) |
| M4 × 0.7 | 5.41 mm (0.213 in) | 1.0 mm (0.039 in) | 7.87 mm (0.310 in) | 6.9 mm (0.27 in) |
| M5 × 0.8 | 6.35 mm (0.250 in) | 1.0 mm (0.039 in) | 8.64 mm (0.340 in) | 7.1 mm (0.28 in) |
| M6 × 1 | 8.75 mm (0.344 in) | 1.4 mm (0.055 in) | 11.18 mm (0.440 in) | 8.6 mm (0.34 in) |
| M8 × 1.25 | 10.5 mm (0.413 in) | 1.4 mm (0.055 in) | 12.7 mm (0.500 in) | 9.7 mm (0.38 in) |
M5 nuts in this table are the SS and CLSS types, which the bulletin lists for that thread. The inch figures are conversions; the bulletin prints its own inch table for unified threads.
No Deburring and No Chamfer
On a laser-cut or punched panel, the instinct is to break the hole edge. PEM’s instructions say the opposite: deburring on either side of the sheet removes the metal needed for clinching. The Machine Design article sets a numeric limit, no chamfer or broken edge over 0.127 mm (0.005 in).
For a buyer, the practical consequence is a drawing note. Holes for clinch hardware are excluded from any general deburring instruction, so the person running the deburring machine leaves them alone.
Edge Distance and Spacing
The edge distance in Table 3 is the shortest distance from the hole’s center to the sheet edge. Closer than that, the edge bulges during the squeeze, and once it bulges the metal no longer fills the undercut. PEM allows an exception only where a special fixture restrains the edge. Two fasteners near each other follow a simple formula from the Machine Design article: the distance between holes equals the first fastener’s centerline-to-edge value plus half the diameter of the second hole.
Take two M6 nuts. The spacing comes to 8.6 mm plus half of 8.75 mm, about 13.0 mm (0.51 in) between centers, before any allowance for tolerance or for the screws that go into them.
Bends follow the same logic. PEM refers designers to its tech sheet on centerline-to-edge distance for proximity to bends, and its bulletin footnote keeps fasteners away from bends and other highly cold-worked areas, which are both harder and already strained.
Holes the Nut Makes Itself
One exception removes the hole step. PEM’s tech sheet on self-piercing tooling lets an S nut with a code 2 shank pierce its own hole during installation, under narrow conditions: aluminum sheet no harder than HB 79.7 (HRB 40), 1.5 to 2.0 mm (0.059 to 0.079 in) thick, and only the 1/4-20, 5/16-18, M6 and M8 threads. A raised ring on a special anvil pierces the slug and embosses the panel so the nut sits sub-flush on the shank side. The tech sheet lists installation forces of 49 to 67 kN (11,000 to 15,000 lbf) for this method in 5052-H34, well above the conventional figures, and recommends a fixture or template to locate the nut where no die is used.
Finishing Order for Plated, Painted and Anodized Panels
Clinching is the last metal-forming step on the panel, and the finish comes before it. The ASSEMBLY article puts plating, finishing and anodizing before the fasteners go in, and PEM’s list adds two specific cautions. Steel or stainless fasteners are not to go into aluminum panels before anodizing or finishing, and no fastener goes in on the pre-painted side of a panel.
The reasons are practical. An anodizing or plating bath would attack or coat the fastener, and a coating applied over an installed nut can fill its threads. Where a panel has to be powder coated after hardware is in, PEM offers PreTect thread masking plugs, fitted at the factory and ordered with a TP suffix, which protect the threads through the paint or powder coating process.
Galvanic pairing is the other finishing question. The Machine Design article notes that passive 300 series stainless and aluminum sit some distance apart in the galvanic series, so corrosion at the interface is possible where an electrolyte and oxygen are present. Its preferred alternatives, in descending order, are an aluminum fastener strong enough for the job, a plated 300 series part, or a zinc-plated or special stainless part, depending on the alloy.
- Anodized aluminum panel: anodize first, then install, and choose the fastener material with the galvanic question settled.
- Plated steel panel: plate first, then install; the bulletin’s unplated threads are sized to accept a go gauge after 0.0064 mm (0.00025 in) of plating.
- Powder coated panel with hardware already in: order masked threads, and expect the coating to be kept off the clinch face.
- Pre-painted coil or sheet: install from the unpainted side, as PEM’s guidance requires.
Settling the finishing order on the drawing costs one note. Getting it wrong costs either a stripped coating round every nut or a batch of threads full of powder.
Press Force and Parallel Tooling for the Squeeze
Any parallel-acting press with adjustable force can do the work, according to the Machine Design article, and the ASSEMBLY article lists manual, pneumatic and servo presses as long as the throat is deep enough to reach the installation point. What no press can do is replace the squeeze with an impact. A hammer blow does not give the sheet time to flow into the undercut, and PEM’s guidance rules it out under any circumstances.
Punch, Anvil and Seating
The nut sits in an anvil with a counterbore or protrusion sized to it, and a flat punch closes on the sheet. For PEM’s M4, M5 and M6 nuts, the recommended anvils have a cavity of 8.38, 9.17 and 11.53 mm (0.330, 0.361 and 0.454 in), held to ±0.05 mm. The force goes through the head and into the sheet, never through the thread. For the miniature FE nuts, PEM specifies a cavity in either punch or anvil so the load lands on the knurled collar and not on the barrel.
Installation is complete when the head meets the sheet squarely and the clinching ring is embedded around its whole circumference. On some fasteners the mark of completion is a head flush with the panel. PEM’s miniature FE nuts have two end points: the knurled collar flush with the top of sheets 1.5 mm (0.060 in) and thicker, or the shank flush with the bottom of sheets 1.0 to 1.5 mm (0.040 to 0.060 in).
Installation Force by Sheet
PEM prints installation forces as general reference and asks that the optimum force be found by test before a production run. For its nuts with a code 1 shank, the bulletin lists the force alongside the average pushout and torque-out the installed nut then gave:
- M4 S or CLS nut in 5052-H34 aluminum: 11.2 to 13.4 kN (2,520 to 3,010 lbf); pushout 470 N (106 lbf), torque-out 2.6 N·m (23 in·lbf).
- M4 S or CLS nut in cold-rolled steel: 18 to 27 kN (4,050 to 6,070 lbf); pushout 645 N (145 lbf), torque-out 4.0 N·m (35 in·lbf).
- M6 S or CLS nut in 5052-H34 aluminum: 18 to 32 kN (4,050 to 7,190 lbf); pushout 1,580 N (355 lbf), torque-out 10.2 N·m (90 in·lbf).
- M6 S or CLS nut in cold-rolled steel: 27 to 36 kN (6,070 to 8,090 lbf); pushout 1,760 N (396 lbf), torque-out 17 N·m (150 in·lbf).
- M6 SP nut in 304 stainless: 60 kN (13,490 lbf); pushout 2,000 N (450 lbf), torque-out 17 N·m (150 in·lbf).
- M6 SH nut in 2.5 mm S700MC at HRC 23: 52.1 kN (11,710 lbf); pushout 4,200 N (944 lbf), torque-out 17 N·m (150 in·lbf).
Over-squeezing has its own signature. PEM lists a crushed head, distorted threads and a buckled sheet. Under-squeezing leaves a visible gap under the head and a ring that is only partly embedded. Between those two, the press setting is a matter of the sheet in hand, and that is why the maker’s table is treated as a starting value.
The table gives a range. Each material lot’s first panel gives the setting.
Automated Feeding
For larger quantities, the ASSEMBLY article describes presses that feed fasteners into punched or drilled holes and seat them with a parallel squeeze, at feed rates up to six times those of manual insertion, with the squeeze adjustable for variation in sheet thickness and hardness and in fastener height. One handling system it describes inserts up to four different fasteners in a single handling of a part. The quantity at which that becomes worthwhile depends on the hardware count per panel more than on the panel count.
Pushout and Torque-Out Tests on the First Panel
Three tests describe an installed fastener, in the Machine Design article’s account. Torque-out measures resistance to turning in the panel, pushout measures axial resistance to being pushed out of the sheet, and pull-through measures resistance to being pulled through the sheet under clamping torque. The same article puts pushout at roughly 5 to 10 % of the installation force, which matches the M6 figures above: 1,760 N against 27 to 36 kN is 5 to 7 %.
PEM’s bulletin describes how its own figures were taken. Pushout is applied from the shank side with a hardened test screw of grade 5 or better, the sheet supported round the fastener on a hardened bushing, at about 6.35 mm (0.25 in) per minute. Torque-out is applied from the head side with a hardened screw and washer while the strip is held firmly, with at least two screw threads beyond the fastener.
The pushout and torque-out figures listed with the forces above are averages under the maker’s conditions. Torque-out for the M6 steel nut is the same 17 N·m in cold-rolled steel, in 304 stainless and in S700MC, while pushout climbs from 1,760 to 4,200 N (396 to 944 lbf) as the sheet gets harder and the nut changes to suit it. PEM states that variations in hole size, sheet material and installation procedure affect performance and recommends testing in the actual application.
Reading a Rejected Installation
Most faults are visible before any load is applied. A ring of bright, undisturbed sheet round the head means the clinching ring did not embed.
Where the sheet is raised or dished, it buckled under excess force. If the nearest edge bulges, the edge distance was too small. Any screw that binds on the first turns means the thread was distorted, usually by force through the shank. Each of these points back to a step in Table 1.
The direction of load matters as well. PEM advises installing the mating screw from the side opposite the head, so the fastener load acts toward the sheet. The clinch is designed to hold the nut during handling and to resist torque during assembly, not to carry the joint’s load away from the panel.
What a First Article Record Holds
A first panel record for clinch hardware notes the fastener part number and shank code, the sheet grade, thickness and measured hardness, the hole size as cut, the press and its force setting, and the pushout and torque-out results on sacrificial coupons from the same lot. That record lets a second lot of sheet be checked against the first, which matters because the press setting belongs to the material. Small first runs of panels with clinch hardware suit low-volume sheet metal, and a panel that settles into repeat orders carries its first-article force setting and test record into bridge production.
How far the published averages hold for a sheet at the top of its hardness band, or for a nut placed at exactly its minimum edge distance, is a question each maker leaves to the user’s own test.
Sources and Further Reading
- Self-Clinching Nut Fastener Installation Do’s and Don’ts, PEM (PennEngineering)
- CL Self-Clinching Nuts, Bulletin CL, 2026, PennEngineering
- FE Miniature Self-Clinching Fasteners, Bulletin FE, 2026, PennEngineering
- Tech Sheet PEM REF, Self-Piercing, Self-Clinching Tooling, July 2019, PennEngineering
- Self-Clinching Fasteners, ASSEMBLY, September 2018, reprint, ASSEMBLY magazine (BNP Media), hosted by PEM
- The Basics of Self-Clinching Fasteners, 10 July 2008, Machine Design