A 1 mm (0.039 in) stainless sheet cut with nitrogen on a 12 kW fiber laser runs at 50 to 60 m/min (about 2,000 to 2,400 in/min), according to the parameter tables GWEIKE publishes for its M-Series machines. A 20 mm (0.79 in) stainless plate on a 6 kW machine of the same family moves at 0.2 to 0.35 m/min, which is 8 to 14 in/min. Same gas and same alloy family, and the feed rate differs by a factor of roughly 150 to 300.
The gas is what holds that range together, and it is also what decides how the edge looks, whether it takes paint, and how much finishing the part needs afterward. A cut is not only light. Along the beam’s axis a jet of gas leaves the nozzle, and it either burns the steel or simply blows molten steel out of the slot. The sections below follow the choice of gas from the sheet to the edge, with the figures the makers and the gas suppliers print.
Which Assist Gas Cuts Which Sheet Metal
Three gases cover almost all sheet work: oxygen, nitrogen and compressed air. Oxygen belongs to carbon and low-alloy steel, nitrogen to stainless steel and aluminum, and air sits between them as the cheaper trade for thin parts that tolerate a slightly darker edge. The reason is chemical before it is mechanical.
Oxygen is active. Linde describes it as burning and vaporizing the metal, with the reaction adding heat to the cut. Nitrogen is inert, so it melts nothing by itself and carries no extra heat; the beam does all the melting, and the gas momentum throws the melt out of the kerf. Trumpf names the two modes flame cutting (oxygen) and fusion cutting (nitrogen or argon).
| Gas | Sheet it suits | Pressure the makers print | Edge it leaves | Source |
|---|---|---|---|---|
| Oxygen | Carbon and low-alloy steel | up to 6 bar (87 psi) for flame cutting; under 1 bar (15 psi) above 20 mm (0.79 in) thick | Oxide-coated, scaled edge | Trumpf; Linde |
| Nitrogen | Stainless steel, aluminum, brass | 2 to 20 bar (29 to 290 psi) for fusion cutting; roughly 10 to 15 bar (145 to 218 psi) for thick sheet | Metallic, scale-free edge | Trumpf; Linde |
| Compressed air | Thin carbon steel, stainless, aluminum | 10 to 16 bar (145 to 232 psi) on thin carbon steel in GWEIKE’s table | Darker, oxidized edge on stainless; more dross on aluminum | GWEIKE; Air Liquide |
Read the third row with care. Compressed air is about four-fifths nitrogen and one-fifth oxygen, so it behaves like a weak oxygen cut on the way through. The laser cutting guide from Air Liquide says an air-cut stainless edge shows an oxidized appearance where a nitrogen cut stays smooth, and that air produces more dross on aluminum alloy. Where the part will be seen, anodized or welded next, that difference matters more than the saving.
Oxygen burns the steel and leaves a scaled edge. Nitrogen only blows melt out and leaves metal bright. Air does a little of both.
Oxygen Cutting of Carbon Steel and What Its Edge Does Later
Oxygen cuts thick carbon steel at low pressure. Linde gives about 20 bar as the ceiling for the thinnest sheet of 2 to 3 mm (0.08 to 0.12 in) and says pressure above 20 mm thickness is rarely over 1 bar gauge. Too much pressure drives sideways burning, which shows up as heavy dross or a cut that does not go through. GWEIKE’s tables use 0.5 to 0.7 bar (7 to 10 psi) for most thicknesses, and 1.0 to 1.5 bar (15 to 22 psi) from 25 mm.
| Thickness | 6 kW speed | 12 kW speed | Focus position | Gas pressure |
|---|---|---|---|---|
| 6 mm (0.24 in) | 2.7 to 3.2 m/min (106 to 126 in/min) | not listed | +4 mm above the surface | 0.5 to 0.7 bar (7 to 10 psi) |
| 10 mm (0.39 in) | 2.0 to 2.3 m/min (79 to 91 in/min) | 2.0 to 2.3 m/min (79 to 91 in/min) | +3 to +4 mm | 0.5 to 0.7 bar (7 to 10 psi) |
| 16 mm (0.63 in) | 1.2 to 1.4 m/min (47 to 55 in/min) | 2.8 to 3.0 m/min (110 to 118 in/min) | +3 to +6 mm | 0.5 to 0.7 bar (7 to 10 psi) |
| 25 mm (0.98 in) | 0.4 to 0.5 m/min (16 to 20 in/min) | 0.8 to 1.0 m/min (31 to 39 in/min) | +3 to +11 mm | 1.0 to 1.5 bar (15 to 22 psi) |
Two lessons sit in the table. At 10 mm the extra power buys nothing, since the burning reaction and not the beam sets the pace. From 16 mm up the larger machine pulls ahead, because a wide kerf needs the energy to keep the front of the cut molten. The focus sits above the surface for oxygen, the opposite of what nitrogen wants, and a nozzle with a smaller bore than the nitrogen nozzle suits it, according to the trade article in All About Industries.
One consequence of the edge shows up later. That same article says oxygen edges are scaled and need rework on parts going to painting or galvanizing. Discoloration, oxidation and slag become typical on thick sheet, from about 20 mm (0.8 in).
A part that gets powder coated after cutting needs the oxide layer removed, or the cut done in nitrogen. Welded at the cut edge, a part carries oxide into the weld pool unless the edge is cleaned. Only a part that stays hidden, such as a bracket painted black, can take the oxide edge as it comes.
The decision therefore reaches back from the finish to the gas, and it is cheapest to make it before the nesting file is released.
Nitrogen Cutting of Stainless Steel and Aluminum
Nitrogen cuts at many times the pressure oxygen uses, because it has to do the whole job of clearing the slot. Linde states that thick mild and stainless sheet cut best at roughly 10 to 15 bar (145 to 218 psi), and Trumpf prints 2 to 20 bar (29 to 290 psi) for fusion cutting in general. The All About Industries article puts flow at about 90 m³/h when thick stainless is cut, which is why a shop that runs nitrogen all day buys it by the tank farm and not by the cylinder.
Purity matters at the edge, and the numbers are specific. Linde says very thick stainless often needs at least 99.995 percent nitrogen, and its own laser grade is rated at 99.998 percent. Oxygen contamination causes yellowing of the cut edge and dross that is hard to remove, and the effect grows when a slow cut gives the reaction more time.
| Thickness | 3 kW speed | 6 kW speed | 12 kW speed | Focus position | Pressure |
|---|---|---|---|---|---|
| 1 mm (0.04 in) | 28 to 35 m/min | 40 to 50 m/min | 50 to 60 m/min | 0 mm | 10 to 12 bar |
| 3 mm (0.12 in) | 7 to 10 m/min | 15 to 18 m/min | 30 to 35 m/min | -1.5 mm | 10 to 12 bar |
| 6 mm (0.24 in) | 2.0 to 2.7 m/min | 6 to 7 m/min | 13 to 15 m/min | -3 mm | 10 to 12 bar |
| 10 mm (0.39 in) | 0.5 to 0.6 m/min | 1.6 to 2.0 m/min | 6.5 to 7.5 m/min | -6 mm | 16 to 20 bar |
| 20 mm (0.79 in) | not listed | 0.2 to 0.35 m/min | 1.2 to 1.4 m/min | -11 to -12 mm | 16 to 20 bar |
Convert any row by multiplying m/min by 39.4 for inches per minute; the 3 mm row at 6 kW, for example, is 590 to 710 in/min. The pressure column is GWEIKE’s own, 10 to 12 bar for thin sheet rising to 16 to 20 bar for thick sections, and the page adds that every figure should be fine-tuned by 10 percent for the alloy, the surface and the temperature of the shop.
Aluminum follows the same pattern with different speeds. At 12 bar for thin sheet, rising to 18 to 20 bar from 10 mm, the same tables list a 3 mm aluminum sheet at 25 to 30 m/min on 12 kW and 14 to 16 m/min on 6 kW. The speeds are close to stainless in the thin range and fall away more slowly in the thick range.
Focus moves downward as the sheet thickens. At zero for 1 mm it falls to roughly 6 mm below the surface at 10 mm, so the beam waist sits low in the slot and the melt leaves from the bottom.
Stainless wants nitrogen at 10 to 20 bar and a focus that sinks as the sheet thickens. A thick cut at 12 kW runs about four times as fast as at 6 kW.
Compressed Air as a Third Gas for Thin Sheet
Air is the gas a shop uses when volume is high and the edge is allowed to be less than perfect. GWEIKE lists carbon steel under a combined heading of nitrogen or air, at 10 to 16 bar (145 to 232 psi), with nozzles from 1.5 to 3.5 mm and speeds for 1 mm sheet that reach 35 to 45 m/min on 6 kW and 50 to 60 m/min on 12 kW. The Bodor guide recommends air for thin stainless, carbon steel and aluminum.
That saving has a visible price. Air Liquide ties the oxidation of a stainless edge to thickness: as the sheet gets thicker, the air-cut edge looks worse, while nitrogen stays smooth. Aluminum cut with air shows more dross.
Air Liquide also lists a blend of nitrogen with 5 percent oxygen for low-alloy steel, a middle step between the two pure gases. The blend exists because pure nitrogen on thicker carbon steel is slow, and pure oxygen leaves the heaviest oxide.
- Use air when the part is thin, hidden or will be ground or blasted afterward.
- Nitrogen suits stainless or aluminum parts whose edge will be seen, welded, anodized or powder coated.
- Oxygen suits thick carbon steel, where the oxide layer is removed or painted over.
Piercing, Lead-ins and Where the Cut Begins
Every internal contour starts with a hole. The pierce is a separate step with its own power, frequency, nozzle height and gas, and on thick plate it takes seconds, not fractions of one. GWEIKE prints one example, a 22 mm carbon steel pierce on 3 kW with oxygen, built in three stages.
The first stage runs at 100 percent duty and 200 Hz with the nozzle high at 12 mm (0.47 in), oxygen at 1.0 bar (15 psi) and focus at 0 mm, for 200 ms plus a 200 ms purge. Next the median stage drops to 45 percent duty at 150 Hz, nozzle at 8 mm (0.31 in), 0.7 bar (10 psi), focus at -4 mm, and holds for 2,500 ms. The low stage runs 55 percent duty, nozzle at 4 mm (0.16 in), 0.6 bar (9 psi), focus at -6 mm and 3,000 ms.
The guide calls these figures reference data and tells the operator to run a test pierce on scrap first. That is a fair statement of the limit. A pierce on thick plate sprays molten metal back up toward the lens, so the nozzle rises first and descends as the hole opens. Nozzle standoff in normal cutting, by contrast, is small, and Bodor puts it at 0.5 to 2.0 mm (0.02 to 0.08 in).
A buyer can read two things from this. Hole count drives cycle time on thick sheet, because every pierce costs seconds, and a nest with hundreds of small holes in 16 mm plate is slower than the contour length suggests. Pierce location also decides where dross and heat collect, so a sound programmer starts the cut in scrap, away from a finished edge, and joins it to the contour with a lead-in.
Reading the Edge Left by the Cut
The edge records what the gas and speed did. Trumpf describes drag lines that run nearly parallel to the beam at low cutting speed and bend away from the beam as speed climbs. It adds that a wrong cutting speed raises surface roughness and causes burr.
Burr and dross are different defects. A burr is a thin lip on the bottom edge, from melt that cooled before it left. Dross is a thicker, beaded residue, harder to remove, from too little pressure or too slow a cut. The All About Industries article reports shop experience that lowering oxygen pressure by 0.1 bar often removes burnt corners, and raising nitrogen pressure by 0.5 bar often removes burrs. It also notes that nitrogen cuts on fiber lasers leave fiber burrs that call for deburring.
- Look at the bottom edge first, since burr and dross collect there.
- Check inside corners and small holes, where heat builds and oxygen cuts burn out.
- Run a fingernail along the edge; a stainless nitrogen cut feels smooth where an air cut feels gritty.
- Compare the color: bright metal means nitrogen with low oxygen, straw yellow means oxygen contamination, dark gray means oxide.
Kerf is small and does not need its own tolerance in most parts. Trumpf says the focal spot is often below 0.5 mm (0.02 in) and the kerf barely wider than the focused beam, so the programmer compensates for it in the nest and the buyer sees it only on tight mating cutouts.
The edge colour is a record of the gas. Bright metal came from clean nitrogen, yellow from oxygen leaking in, and dark gray from oxygen or air doing the cutting.
What to State on the Order for Laser Cut Sheet Parts
Gas does not appear on most drawings, yet it decides downstream cost, so it belongs in the request. A short statement removes a round of questions and keeps edge finish from becoming a dispute at inspection.
- Name the material and thickness, and the finish that follows (powder coat, anodize, weld, none).
- State whether an oxide edge is acceptable, and on which edges.
- State whether burr is removed, and to what radius or feel.
- Call out edges that mate, since kerf compensation and edge condition both reach them.
- Ask for first-piece confirmation of edge color on stainless and aluminum.
Parts that begin as a few cut sheets and then grow into a few hundred can move through low-volume sheet metal fabrication and on into bridge production with the same gas choices carried forward, so the edge a buyer approved at the first piece is the edge that ships on the last.
Sources and Further Reading
- GWEIKE, Parameter Guide, Fiber Laser Cutting (M-Series cutting tables and pierce example). https://gwklaser.com/fiber-laser-cutting-parameters-guide.html
- Linde, Laser Cutting with LASERLINE (oxygen and nitrogen purity and pressure). https://www.linde-gas.com/processes/thermal-cutting/laser-cutting
- All About Industries, Cutting Gas in Laser Cutting: How Oxygen and Nitrogen Shape the Cutting Edge. https://www.all-about-industries.com/how-oxygen-and-nitrogen-shape-the-cutting-edge-a-0998ffea9af2d4989ab8302169e219e5/
- Trumpf, Laser Cutting application page (flame and fusion cutting, kerf, pressures). https://www.trumpf.com/en_GB/applications/laser-cutting/
- Bodor, 5 Key Parameters for Fiber Laser Cutting (nozzle diameter and standoff). https://www.bodor.com/en/blogs/5-Key-Parameters-for-Fiber-Laser-Cutting.html
- Air Liquide Singapore, Laser Cutting (gas choice by material). https://sg.airliquide.com/sites/al_sg/files/2026-03/laser-cutting.pdf