The technical data sheet for IGP-DURA mix 3303E-A1, a matte powder sold for indoor use, gives its cure as 10 to 15 minutes at an object temperature of 190 °C (374 °F). The same sheet lists condensation water and salt spray resistance at 500 to 1,000 hours. A coat is finished in a quarter of an hour, and the test that proves it takes weeks, so no lot is ever released on the corrosion figure itself.
For a buyer, a powder coated batch has two clocks. One runs in minutes, through the oven, and the other runs in stages of preparation, cooling and checking that depend on what is hung on the rack. The sections below follow a batch of sheet metal parts through the coater’s line and put numbers where the makers print them.
The Stages a Coated Batch Passes Through
A batch of sheet metal parts goes through six stages on its way from the bare part to a coated one: pretreatment, drying, masking and hanging, application, cure, and cooling and packing. Each stage has a condition the powder maker states, and each has its own place in the schedule.
| Stage | What is done | Published condition | Source |
|---|---|---|---|
| Pretreatment | Remove oil, grease and oxidation; convert the surface | Aluminum: chromating to DIN EN 12487, pre-anodization or chrome-free pretreatment per GSB International and QUALICOAT. Steel: zinc or iron phosphating. Galvanized steel: zinc phosphating, chrome (III) passivation or chromating | IGP |
| Drying | Remove moisture and solvents | A maker recommends, but does not require, about 30 minutes at 450 °F (232 °C) for degassing and static discharge on bare parts | Prismatic Powders |
| Masking and hanging | Plug mating surfaces and holes; hang with clean metal-to-metal contact | Contact is needed for a true earth ground; parts are hung so they do not bump one another | Prismatic Powders |
| Application | Electrostatic spray of powder | Film of 60 to 80 µm (0.0024 to 0.0031 in) | IGP |
| Cure | Melt, flow and cross-link | 180 °C for 15 to 25 minutes; 190 °C for 10 to 15; 200 °C for 8 to 12 | IGP |
| Cooling and packing | Cool, then pack without plasticizers | Pack after cooling; store out of the weather | IGP |
IGP adds that the pretreatment has to suit the substrate and the corrosion protection wanted, and that the coater should test the suitability in advance, with a boiling water test followed by a cross-cut adhesion and tape test as the minimum for aluminum and galvanized parts. The sheet also says the coater should run practical trials with the actual object and curing oven.
The cure is a quarter of an hour. Everything before it decides whether the quarter of an hour counts.
Cure Window and the Mass on the Rack
Powder cures by the temperature of the part and not the air in the oven. Prismatic Powders puts it plainly: the thickest portion of the substrate has to reach cure temperature before the timer starts, and when several layers are applied, the substrate takes longer to reach it. IGP’s schedule is written for the object temperature.
| Object temperature | Minimum time | Maximum time | Width of the window |
|---|---|---|---|
| 180 °C (356 °F) | 15 minutes | 25 minutes | 10 minutes |
| 190 °C (374 °F) | 10 minutes | 15 minutes | 5 minutes |
| 200 °C (392 °F) | 8 minutes | 12 minutes | 4 minutes |
Read across, the hotter the cure, the shorter and narrower the window. At 200 °C a part has four minutes of tolerance between under-cure and over-cure. A rack that mixes a 1 mm panel and a 6 mm bracket cannot give both the same time at temperature, since the thick one lags, and the thin one is soaked longer than the sheet allows while the thick one is brought up.
IGP’s own advice is to determine the best conditions by practical trials with the object and the oven. In a batch of sheet metal parts, that advice reduces to a rule: hang parts of similar thickness together.
A part in a thick section is also the slowest to cool. After the oven, parts are cooled before packing, since IGP wants them packed after cooling in materials free of plasticizers.
- Group parts by thickness before they go on the rack.
- Let the thickest part on the rack set the oven time.
- Cooling to ambient comes before stacking or wrapping.
Film Thickness and the Parts That Have to Fit
A film of 60 to 80 µm sits on every face the powder reaches. IGP states 60 to 80 µm as the recommended film thickness, and adds that textured coatings or differences in hiding power may need more. Prismatic gives 2 to 3 mils (51 to 76 µm) per coat for most of its powders.
On a sheet metal part that thickness takes room. A tab 3 mm wide carries film on both faces, so it grows by 2 × 60 to 2 × 80 µm, which is 0.12 to 0.16 mm (0.005 to 0.006 in). The slot it enters loses the same amount from its two walls. A round hole of 5 mm shrinks in diameter by the same 0.12 to 0.16 mm, since the film lines the whole circle. Those figures are the writer’s arithmetic from IGP’s film range, not an allowance a maker states.
Prismatic warns that improper masking on mechanical parts or mating surfaces may cause tolerance or functionality issues. A threaded hole, a grounding point and a surface that mates with another part are masked, or left as drawn dimensions that allow for film.
The quantity of powder is also a figure the sheet gives. IGP lists a density of 1.3 to 1.6 kg/l for this powder and a film of 60 to 80 µm. One kilogram of powder at 1.45 kg/l is about 0.69 l, and spread over a film of 70 µm it covers about 9.9 m² (107 ft²), before any powder is lost. The range across the stated density and film runs from about 7.8 to 12.8 m² per kilogram.
For the 130 blanks of 180 by 110 mm from the nesting piece in these resources, the two faces of a blank carry 0.0396 m², and a sheet’s worth carries about 5.1 m². That is 0.4 to 0.66 kg of powder at theoretical coverage. The number matters less for the powder than for what it shows: coating time follows the surface area on the rack, not the count of parts.
Mixed Substrates on One Order
An assembly often has parts in more than one base metal, a steel frame with an aluminum cover, or a galvanized back panel. IGP’s pretreatment list is written per substrate, and the three do not share a line: aluminum takes chromating to DIN EN 12487, pre-anodization or a chrome-free system to the GSB International and QUALICOAT specifications; steel takes zinc or iron phosphating; galvanized steel takes zinc phosphating, chrome (III) passivation or chromating.
The same aluminum line also takes the parts that are not sheet. A frame cut from aluminum extrusion and the panels it carries go through one pretreatment, which is why an enclosure built from both is often coated on one order and matched in one color.
Stainless steel does not appear in IGP’s list at all, so a coater is asked how a stainless part is prepared before it is accepted into a coated batch. The same applies to any alloy the sheet does not name.
For a run, the consequence is in the schedule. A batch with three substrates is three pretreatment sets that arrive at one powder booth, and the parts then meet again on the rack or in the cure oven. Where a coater runs aluminum on one day and steel on another, a three-substrate order can take three visits, and the last part sets the date of the whole order.
The galvanized case adds a surface that was finished before the coater saw it. A hot-dip coating of G90, per the GalvInfo note, adds about 42 µm of total thickness to a steel sheet, and the powder film of 60 to 80 µm sits on top of that. The two together are the thickness a tab and a slot see. IGP’s minimum requirement for galvanized and aluminum parts, a boiling water test with a cross-cut adhesion and tape test, reads as a warning that these substrates hold coatings less forgivingly than bare steel.
Sizing the Powder and the Rack for a Batch
A batch is planned by surface, because powder is applied per square meter. IGP packs this powder in 20 kg cartons and in 500 kg containers of 25 liners of 20 kg each. At the theoretical coverage of 7.8 to 12.8 m² per kilogram, one carton covers 156 to 256 m². For the 130 blanks of the nesting example at 5.15 m² per sheet, a carton covers 30 to 50 sheets of such blanks, before the losses of real application.
Two things limit a rack before the powder does. One is the oven: parts are hung so they do not touch, per Prismatic, and each needs a clean metal-to-metal contact to ground. The other is the cure itself, since a rack of heavy parts takes longer to come up to the object temperature than a rack of light ones, and the timer starts only then.
A planner who wants a day count has to ask the coater for the rack size and the oven cycle. The figures in this piece do not produce days, because none of the published sheets prints a line speed or a rack capacity, and a figure of that kind belongs to the coater’s own line.
Inspection of a Coated Lot
The data sheet lists the tests its film passes, on steel 0.5 mm thick with a 60 to 80 µm film cured at 190 °C for 10 minutes. These are results on a test panel under one cure, and a lot is judged on a few of them.
| Property | Value | Test |
|---|---|---|
| Gloss at 60 degrees | 25 to 35 | DIN EN ISO 2813 |
| Cross-cut adhesion | Gt 0 | DIN EN ISO 2409 |
| Mandrel bend | 5 mm (0.2 in) or less | DIN EN ISO 1519 |
| Impact | 10 inch-pounds (1.1 J) or more | ASTM D 2794 |
| Cupping | 5 mm (0.2 in) or more | DIN EN ISO 1520 |
| Buchholz hardness | 80 or more | DIN EN ISO 2815 |
| Condensation water | 500 to 1,000 hours, no infiltration or blisters | DIN EN ISO 6270-2 |
| Salt spray | 500 to 1,000 hours, no infiltration or blisters | DIN EN ISO 9227 |
The impact figure converts at 0.113 J per inch-pound, which is the writer’s arithmetic. IGP marks the corrosion hours as depending on pretreatment, and it notes limited resistance to organic solvents and an indoor quality classification for this grade.
Three kinds of check belong to a lot. The first is look: color and gloss against an approved sample, in good light. Second comes film thickness, measured on the parts with a gauge, so the 60 to 80 µm band is confirmed on the faces that matter. Third comes adhesion, by cross-cut and tape on a part or a sample that went through the same line.
Corrosion tests belong to the qualification of the powder and its pretreatment. A buyer who needs a corrosion figure asks for the pretreatment and the powder’s tested system, and does not expect a 1,000 hour salt spray on each lot.
Gloss, film and adhesion are checked on the lot. Corrosion hours belong to the system the lot was made with.
Color, Powder Lots and Repeat Orders
Color is where a coated batch meets the buyer’s eye, and where a repeat order is judged. A drawing that names a RAL number fixes the shade on paper, and the approved first piece fixes it on metal. Both are kept, since gloss, texture and the metal beneath shift how the same powder looks on a given part. A repeat order therefore quotes the drawing’s color and also the approved piece it is compared with, and the buyer keeps that piece where it can be handed over.
Powder keeps. IGP gives a storage life of at least 24 months at 25 °C or below in an unopened original container, so a powder of one batch can be held for a repeat order. Its particle size is under 100 µm and its solids above 99 percent. Colors are RAL, with metallic and individual colors on request.
The practical effect is that a second order can be made with the same powder lot as the first, or not. A repeat batch from a new powder lot is a color check against the first approved piece.
IGP also says small portions of recovered powder can be added to fresh powder, with overspray kept to a minimum, which means the powder on a part is not always virgin. Prismatic adds that metallic coatings need 3 to 5 extra minutes after the flash phase to set the metallic in place, so a metallic color has a schedule of its own.
Packing, Storage and Release
The release of a coated lot is a short step with several things to count. Parts leave the oven warm, and the rack comes apart as they cool, so the order of unloading is also the order of packing. A lot that is cooled in one place and packed in another keeps its identity only if the rack tags travel with it.
After cure the parts are cooled and packed. IGP says coated parts should be packed after cooling with materials free of plasticizers and stored protected from the weather, so condensation does not leave water spots. It refers cleaning to RAL-GZ 632 or SZFF 61.01.
A cured film is hard but not immune to what touches it. IGP’s advice on cooling before packing, plasticizer-free wrap and dry storage is aimed at the marks and spots that arise after the oven, and none of them shows until the box is opened.
- Pack after full cooling, with no plasticizer in the wrap.
- Keep parts apart so no face bears on another.
- Store dry, out of the weather.
- Count the parts against the order before the box is closed.
A batch that starts at a few coated parts and grows to hundreds can pass through low-volume sheet metal production and into bridge production with the same pretreatment, cure and inspection record, so the first approved piece is the reference for the last.
Sources and Further Reading
- IGP Powder Coatings, Technical Data Sheet IGP-DURA mix 3303E-A1, TDS 240424 v1.2 (cure, film thickness, pretreatment, tests, storage, packing). https://www.igp-powder.com
- GalvInfo Center, GalvInfoNote 1.1, Understanding Coating Weight Designations for Zinc-Based Coatings on Steel Sheet, Rev 4.0, December 2020 (G90 coating thickness). https://www.galvinfo.com/wp-content/uploads/sites/8/2021/01/GalvInfoNote-1-1-Rev-4-0.pdf
- Prismatic Powders, Application Guide, General Powder (cure by part metal temperature, film per coat, masking, grounding, flash cure). https://images.nicindustries.com/prismatic/documents/2274/prismatic-powders-application-guide-dt20230508192819506132.pdf